Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 7.2 - 7.34 g/cm³ Show Material materials with Dichte of 7.2 - 7.34 g/cm³ | Typical for Malleable Cast Iron |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 23.0 °C | 3 % Show Material materials with Dehnung of 3 % | |
Elastizitätsmodul | 23.0 °C | 179 GPa Show Material materials with Elastizitätsmodul of 179 GPa | |
Härte, Brinell | 23.0 °C | 187 - 241 [-] Show Material materials with Härte, Brinell of 187 - 241 [-] | |
Poissonzahl | 23.0 °C | 0.27 [-] Show Material materials with Poissonzahl of 0.27 [-] | Typical for Malleable Cast Iron |
Schubmodule | 23.0 °C | 64 GPa Show Material materials with Schubmodule of 64 GPa | Typical for Malleable Cast Iron |
Streckgrenze | 23.0 °C | 345 MPa Show Material materials with Streckgrenze of 345 MPa | |
Zugfestigkeit | 23.0 °C | 517 MPa Show Material materials with Zugfestigkeit of 517 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1E-5 - 1.4E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1E-5 - 1.4E-5 1/K | Typical for Malleable Cast Iron |
Schmelzpunkt | 1120 °C Show Material materials with Schmelzpunkt of 1120 °C | Typical for Cast Iron | |
Spezifische Wärmekapazität | 23.0 °C | 460 - 527 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 460 - 527 J/(kg·K) | Typical for Malleable Cast Iron |
Wärmeleitfähigkeit | 23.0 °C | 51 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 51 W/(m·K) | Typical for Malleable Cast Iron |
Chemical properties
Property | Value | Comment |
---|---|---|
Eisen | 93.6 - 96.71 % Show Material materials with Eisen of 93.6 - 96.71 % | balance |
Kohlenstoff | 2.2 - 2.9 % Show Material materials with Kohlenstoff of 2.2 - 2.9 % | |
Mangan | 0.15 - 1.25 % Show Material materials with Mangan of 0.15 - 1.25 % | |
Phosphor | 0.02 - 0.1 % Show Material materials with Phosphor of 0.02 - 0.1 % | |
Schwefel | 0.02 - 0.2 % Show Material materials with Schwefel of 0.02 - 0.2 % | |
Silizium | 0.9 - 1.9 % Show Material materials with Silizium of 0.9 - 1.9 % |
Technological properties
Property | ||
---|---|---|
Application areas | Planet carriers, Certain transmission gears and differential cases. | |
Processing history | as agreed |