Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | Typical for Wrought 4000 Series Aluminium |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Dehnung | 3.0 % Show Material materials with Dehnung of 3.0 % | T86 | ASTM B211 | Bar, Rod, Wire | |
4.0 % Show Material materials with Dehnung of 4.0 % | T86 | ASTM B211 | Bar, Rod, Wire | A50 | |
Elastizitätsmodul | 69.0 - 71.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 71.0 GPa | Typical for Wrought 4000 Series Aluminium | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 4000 Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 4000 Series Aluminium | |||
Schubmodule | 26.0 GPa Show Material materials with Schubmodule of 26.0 GPa | Typical for Wrought 4000 Series Aluminium | |||
Zugfestigkeit | 350.0 MPa Show Material materials with Zugfestigkeit of 350.0 MPa | T86 | ASTM B211 | Bar, Rod, Wire |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.2e-05 - 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.2e-05 - 2.2e-05 1/K | Typical for Wrought 4000 Series Aluminium |
Schmelzpunkt | 520.0 - 630.0 °C Show Material materials with Schmelzpunkt of 520.0 - 630.0 °C | Typical for Wrought 4000 Series Aluminium |
Spezifische Wärmekapazität | 864.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 864.0 J/(kg·K) | Typical for Wrought 4000 Series Aluminium |
Wärmeleitfähigkeit | 138.0 - 155.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138.0 - 155.0 W/(m·K) | Typical for Wrought 4000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 23000000.0 - 30000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 30000000.0 S/m | Typical for Wrought 4000 Series Aluminium |
spezifischer Widerstand | 3.8e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.8e-08 - 5e-08 Ω·m | Typical for Wrought 4000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 Show Material materials with Chrom of 0.1 | T86 | ASTM B211 | Bar, Rod, Wire |
Eisen | 1.0 Show Material materials with Eisen of 1.0 | T86 | ASTM B211 | Bar, Rod, Wire |
Kupfer | 0.5 - 1.3 % Show Material materials with Kupfer of 0.5 - 1.3 % | T86 | ASTM B211 | Bar, Rod, Wire |
Magnesium | 0.8 - 1.3 % Show Material materials with Magnesium of 0.8 - 1.3 % | T86 | ASTM B211 | Bar, Rod, Wire |
Nickel | 0.5 - 1.3 % Show Material materials with Nickel of 0.5 - 1.3 % | T86 | ASTM B211 | Bar, Rod, Wire |
Silizium | 11.0 - 13.5 % Show Material materials with Silizium of 11.0 - 13.5 % | T86 | ASTM B211 | Bar, Rod, Wire |
Zink | 0.25 Show Material materials with Zink of 0.25 | T86 | ASTM B211 | Bar, Rod, Wire |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |