Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 2.65 - 2.7 g/cm³ Show Material materials with Dichte of 2.65 - 2.7 g/cm³ | Typical for Cast 3xx.x Series Aluminium |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Dehnung | 1.0 % Show Material materials with Dehnung of 1.0 % | Class 1, Specimens Cut from Any Area of Casting | ASTM B686 | Casting | |
3.0 % Show Material materials with Dehnung of 3.0 % | Class 1, Specimens Cut from Any Area of Casting | ASTM B686 | Casting | ||
Elastizitätsmodul | 73.0 - 80.0 GPa Show Material materials with Elastizitätsmodul of 73.0 - 80.0 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | |||
Schubmodule | 2.8 GPa Show Material materials with Schubmodule of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Streckgrenze | 205.0 MPa Show Material materials with Streckgrenze of 205.0 MPa | Class 1, Specimens Cut from Any Area of Casting | ASTM B686 | Casting | |
215.0 MPa Show Material materials with Streckgrenze of 215.0 MPa | Class 1, Specimens Cut from Any Area of Casting | ASTM B686 | Casting | ||
Zugfestigkeit | 255.0 MPa Show Material materials with Zugfestigkeit of 255.0 MPa | Class 1, Specimens Cut from Any Area of Casting | ASTM B686 | Casting | |
285.0 MPa Show Material materials with Zugfestigkeit of 285.0 MPa | Class 1, Specimens Cut from Any Area of Casting | ASTM B686 | Casting |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.6e-05 - 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6e-05 - 2.3e-05 1/K | Typical for Cast 3xx.x Series Aluminium |
Schmelzpunkt | 505.0 - 770.0 °C Show Material materials with Schmelzpunkt of 505.0 - 770.0 °C | Typical for Cast 3xx.x Series Aluminium |
Spezifische Wärmekapazität | 960.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 960.0 - 963.0 J/(kg·K) | Typical for Cast 3xx.x Series Aluminium |
Wärmeleitfähigkeit | 130.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 180.0 W/(m·K) | Typical for Cast 3xx.x Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Eisen | 0.2 Show Material materials with Eisen of 0.2 | Class 1, Specimens Cut from Any Area of Casting | ASTM B686 | Casting |
Kupfer | 1.0 - 1.5 % Show Material materials with Kupfer of 1.0 - 1.5 % | Class 1, Specimens Cut from Any Area of Casting | ASTM B686 | Casting |
Magnesium | 0.4 - 0.6 % Show Material materials with Magnesium of 0.4 - 0.6 % | Class 1, Specimens Cut from Any Area of Casting | ASTM B686 | Casting |
Mangan | 0.1 Show Material materials with Mangan of 0.1 | Class 1, Specimens Cut from Any Area of Casting | ASTM B686 | Casting |
Silizium | 4.5 - 5.5 % Show Material materials with Silizium of 4.5 - 5.5 % | Class 1, Specimens Cut from Any Area of Casting | ASTM B686 | Casting |
Titan | 0.2 Show Material materials with Titan of 0.2 | Class 1, Specimens Cut from Any Area of Casting | ASTM B686 | Casting |
Zink | 0.1 Show Material materials with Zink of 0.1 | Class 1, Specimens Cut from Any Area of Casting | ASTM B686 | Casting |