Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.75 g/cm³ Show Material materials with Dichte of 2.75 g/cm³ | T4 | EN 1706 | Casting | |
20.0 °C | 2.75 g/cm³ Show Material materials with Dichte of 2.75 g/cm³ | T4 | EN 1706 |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 80.0 - 110.0 MPa Show Material materials with Bending Fatigue Strength of 80.0 - 110.0 MPa | T4 | EN 1706 | Casting | ||
Elastizitätsmodul | 72.0 GPa Show Material materials with Elastizitätsmodul of 72.0 GPa | T4 | EN 1706 | Casting | ||
20.0 °C | 72.0 GPa Show Material materials with Elastizitätsmodul of 72.0 GPa | T4 | EN 1706 | |||
Härte, Brinell | 90.0 [-] Show Material materials with Härte, Brinell of 90.0 [-] | T4 | EN 1706 | Casting | ||
20.0 °C | 90.0 [-] Show Material materials with Härte, Brinell of 90.0 [-] | T4 | EN 1706 | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 2xx.x Series Aluminium | ||||
Zugfestigkeit | 300.0 MPa Show Material materials with Zugfestigkeit of 300.0 MPa | T4 | EN 1706 | Casting | ||
320.0 MPa Show Material materials with Zugfestigkeit of 320.0 MPa | T4 | EN 1706 | Casting | |||
20.0 °C | 300.0 MPa Show Material materials with Zugfestigkeit of 300.0 MPa | T4 | EN 1706 | |||
20.0 °C | 320.0 MPa Show Material materials with Zugfestigkeit of 320.0 MPa | T4 | EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T4 | EN 1706 | Casting |
100.0 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T4 | EN 1706 | Casting | |
100 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T4 | EN 1706 | Casting | |
Schmelzpunkt | 540.0 - 640.0 °C Show Material materials with Schmelzpunkt of 540.0 - 640.0 °C | T4 | EN 1706 | Casting | |
Spezifische Wärmekapazität | 910.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 910.0 J/(kg·K) | T4 | EN 1706 | Casting | |
20.0 °C | 910.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 910.0 J/(kg·K) | T4 | EN 1706 | ||
Wärmeleitfähigkeit | 20.0 °C | 120.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 120.0 - 150.0 W/(m·K) | T4 | EN 1706 | Casting |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 16000000.0 - 23000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 16000000.0 - 23000000.0 S/m | T4 | EN 1706 | Casting |
spezifischer Widerstand | 4.35e-08 - 6.25e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.35e-08 - 6.25e-08 Ω·m | T4 | EN 1706 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 93.35 % Show Material materials with Aluminium of 93.35 % | T4 | EN 1706 | |
Blei | 0.05 % Show Material materials with Blei of 0.05 % | T4 | EN 1706 | Casting |
Eisen | 0.35 % Show Material materials with Eisen of 0.35 % | T4 | EN 1706 | |
0.35 % Show Material materials with Eisen of 0.35 % | T4 | EN 1706 | Casting | |
Kupfer | 4.2 - 5.0 % Show Material materials with Kupfer of 4.2 - 5.0 % | T4 | EN 1706 | Casting |
Magnesium | 0.15 - 0.35 % Show Material materials with Magnesium of 0.15 - 0.35 % | T4 | EN 1706 | Casting |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | T4 | EN 1706 | Casting |
Nickel | 0.05 % Show Material materials with Nickel of 0.05 % | T4 | EN 1706 | Casting |
Silizium | 0.2 % Show Material materials with Silizium of 0.2 % | T4 | EN 1706 | Casting |
Titan | 0.15 - 0.3 % Show Material materials with Titan of 0.15 - 0.3 % | T4 | EN 1706 | Casting |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | T4 | EN 1706 | Casting |
Zinn | 0.05 % Show Material materials with Zinn of 0.05 % | T4 | EN 1706 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable | |
Corrosion properties | general: not sufficient | |
General machinability | as cast: excellent | |
Processing methods | investment casting, separately cast test sample |