Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.75 g/cm³ Show Material materials with Dichte of 2.75 g/cm³ | F | EN 1706 | Casting | |
20.0 °C | 2.75 g/cm³ Show Material materials with Dichte of 2.75 g/cm³ | F | EN 1706 |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 - 90.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa | F | EN 1706 | Casting | ||
Elastizitätsmodul | 75.0 GPa Show Material materials with Elastizitätsmodul of 75.0 GPa | F | EN 1706 | Casting | ||
20.0 °C | 75.0 GPa Show Material materials with Elastizitätsmodul of 75.0 GPa | F | EN 1706 | |||
Härte, Brinell | 60.0 [-] Show Material materials with Härte, Brinell of 60.0 [-] | F | EN 1706 | Casting | ||
75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | F | EN 1706 | Casting | |||
80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | F | EN 1706 | Casting | |||
20.0 °C | 60.0 [-] Show Material materials with Härte, Brinell of 60.0 [-] | F | EN 1706 | |||
20.0 °C | 75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | F | EN 1706 | |||
20.0 °C | 80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | F | EN 1706 | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | ||||
Schubmodule | 2.8 GPa Show Material materials with Schubmodule of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | ||||
Zugfestigkeit | 150.0 MPa Show Material materials with Zugfestigkeit of 150.0 MPa | F | EN 1706 | Casting | ||
170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | F | EN 1706 | Casting | |||
240.0 MPa Show Material materials with Zugfestigkeit of 240.0 MPa | F | EN 1706 | Casting | |||
20.0 °C | 150.0 MPa Show Material materials with Zugfestigkeit of 150.0 MPa | F | EN 1706 | |||
20.0 °C | 170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | F | EN 1706 | |||
20.0 °C | 240.0 MPa Show Material materials with Zugfestigkeit of 240.0 MPa | F | EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | F | EN 1706 | Casting |
100.0 °C | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | F | EN 1706 | Casting | |
100 °C | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | F | EN 1706 | Casting | |
Schmelzpunkt | 490.0 - 600.0 °C Show Material materials with Schmelzpunkt of 490.0 - 600.0 °C | F | EN 1706 | Casting | |
Spezifische Wärmekapazität | 880.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 880.0 J/(kg·K) | F | EN 1706 | Casting | |
20.0 °C | 880.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 880.0 J/(kg·K) | F | EN 1706 | ||
Wärmeleitfähigkeit | 20.0 °C | 110.0 - 130.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 110.0 - 130.0 W/(m·K) | F | EN 1706 | Casting |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 14000000.0 - 18000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 14000000.0 - 18000000.0 S/m | F | EN 1706 | Casting |
spezifischer Widerstand | 5.56e-08 - 7.14e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.56e-08 - 7.14e-08 Ω·m | F | EN 1706 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 82.55 % Show Material materials with Aluminium of 82.55 % | F | EN 1706 | |
Blei | 0.25 % Show Material materials with Blei of 0.25 % | F | EN 1706 | Casting |
Eisen | 0.8 % Show Material materials with Eisen of 0.8 % | F | EN 1706 | |
0.80 % Show Material materials with Eisen of 0.80 % | F | EN 1706 | Casting | |
Kupfer | 2.0 - 3.5 % Show Material materials with Kupfer of 2.0 - 3.5 % | F | EN 1706 | Casting |
Magnesium | 0.05 - 0.55 % Show Material materials with Magnesium of 0.05 - 0.55 % | F | EN 1706 | Casting |
Mangan | 0.15 - 0.65 % Show Material materials with Mangan of 0.15 - 0.65 % | F | EN 1706 | Casting |
Nickel | 0.35 % Show Material materials with Nickel of 0.35 % | F | EN 1706 | Casting |
Silizium | 7.5 - 9.5 % Show Material materials with Silizium of 7.5 - 9.5 % | F | EN 1706 | Casting |
Titan | 0.25 % Show Material materials with Titan of 0.25 % | F | EN 1706 | Casting |
Zink | 1.2 % Show Material materials with Zink of 1.2 % | F | EN 1706 | Casting |
Zinn | 0.15 % Show Material materials with Zinn of 0.15 % | F | EN 1706 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not recommended | |
Corrosion properties | general: not sufficient | |
General machinability | after thermal treatment: good | |