Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.1 g/cm³ Show Material materials with Dichte of 7.1 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Elastizitätsmodul | 20.0 °C | 78 - 103 GPa Show Material materials with Elastizitätsmodul of 78 - 103 GPa | |
Härte, Brinell | 20.0 °C | 205 - 270 [-] Show Material materials with Härte, Brinell of 205 - 270 [-] | |
Plane-Strain Fracture Toughnes | 20.0 °C | 10.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 10.1 MPa·√m | |
Poissonzahl | 20.0 °C | 0.26 [-] Show Material materials with Poissonzahl of 0.26 [-] | |
Schubmodule | 23.0 °C | 41 GPa Show Material materials with Schubmodule of 41 GPa | Typical for Cast Iron |
Zugfestigkeit | 20.0 °C | 80 - 200 MPa Show Material materials with Zugfestigkeit of 80 - 200 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Schmelzpunkt | 1120 °C Show Material materials with Schmelzpunkt of 1120 °C | Typical for Cast Iron | |
Spezifische Wärmekapazität | 200.0 °C | 460 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 460 J/(kg·K) | |
600.0 °C | 535 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 535 J/(kg·K) | ||
Wärmeleitfähigkeit | 100.0 °C | 52.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 52.5 W/(m·K) | |
200.0 °C | 51 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 51 W/(m·K) | ||
300.0 °C | 50 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 50 W/(m·K) | ||
400.0 °C | 49 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 49 W/(m·K) | ||
500.0 °C | 48.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 48.5 W/(m·K) | ||
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 8E-7 Ω·m Show Material materials with spezifischer Widerstand of 8E-7 Ω·m |