Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 7.75 g/cm³ Show Material materials with Dichte of 7.75 g/cm³ | Typical for Iron Alloy |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 15 % Show Material materials with Dehnung of 15 % | |
Elastizitätsmodul | 23.0 °C | 210 GPa Show Material materials with Elastizitätsmodul of 210 GPa | Typical for Iron Alloy |
Härte, Brinell | 20.0 °C | 120 - 150 [-] Show Material materials with Härte, Brinell of 120 - 150 [-] | |
Poissonzahl | 23.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] | Typical for Iron Alloy |
Streckgrenze | 20.0 °C | 210 - 260 MPa Show Material materials with Streckgrenze of 210 - 260 MPa | |
Zugfestigkeit | 20.0 °C | 390 - 470 MPa Show Material materials with Zugfestigkeit of 390 - 470 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1E-5 - 2E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1E-5 - 2E-5 1/K | Typical for Iron Alloy |
Chemical properties
Property | Value |
---|---|
Kohlenstoff | 3 % Show Material materials with Kohlenstoff of 3 % |
Mangan | 6 - 7 % Show Material materials with Mangan of 6 - 7 % |
Nickel | 12 - 14 % Show Material materials with Nickel of 12 - 14 % |
Phosphor | 0.08 % Show Material materials with Phosphor of 0.08 % |
Silizium | 2 - 3 % Show Material materials with Silizium of 2 - 3 % |