Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 7.15 g/cm³ Show Material materials with Dichte of 7.15 g/cm³ | Typical for Ductile (Nodular) Cast Iron |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 25 % Show Material materials with Dehnung of 25 % | |
Elastizitätsmodul | 23.0 °C | 165 - 180 GPa Show Material materials with Elastizitätsmodul of 165 - 180 GPa | Typical for Ductile (Nodular) Cast Iron |
Härte, Brinell | 20.0 °C | 150 - 180 [-] Show Material materials with Härte, Brinell of 150 - 180 [-] | |
Poissonzahl | 23.0 °C | 0.26 - 0.31 [-] Show Material materials with Poissonzahl of 0.26 - 0.31 [-] | Typical for Ductile (Nodular) Cast Iron |
Schubmodule | 23.0 °C | 63 - 66 GPa Show Material materials with Schubmodule of 63 - 66 GPa | Typical for Ductile (Nodular) Cast Iron |
Streckgrenze | 20.0 °C | 210 - 240 MPa Show Material materials with Streckgrenze of 210 - 240 MPa | |
Zugfestigkeit | 20.0 °C | 440 - 480 MPa Show Material materials with Zugfestigkeit of 440 - 480 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1E-5 - 1.6E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1E-5 - 1.6E-5 1/K | Typical for Ductile (Nodular) Cast Iron |
Max. Betriebstemperatur, lang | -196 - 350 °C Show Material materials with Max. Betriebstemperatur, lang of -196 - 350 °C | ||
Schmelzpunkt | 1150 - 1200 °C Show Material materials with Schmelzpunkt of 1150 - 1200 °C | Typical for Ductile (Nodular) Cast Iron | |
Spezifische Wärmekapazität | 23.0 °C | 460 - 502 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 460 - 502 J/(kg·K) | Typical for Ductile (Nodular) Cast Iron |
Wärmeleitfähigkeit | 23.0 °C | 13 - 42 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 13 - 42 W/(m·K) | Typical for Ductile (Nodular) Cast Iron |
Chemical properties
Property | Value |
---|---|
Kohlenstoff | 2.6 % Show Material materials with Kohlenstoff of 2.6 % |
Mangan | 4 - 4.5 % Show Material materials with Mangan of 4 - 4.5 % |
Nickel | 22 - 24 % Show Material materials with Nickel of 22 - 24 % |
Phosphor | 0.08 % Show Material materials with Phosphor of 0.08 % |
Silizium | 1.5 - 2.5 % Show Material materials with Silizium of 1.5 - 2.5 % |