Allgemein
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 - 90.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa | F | EN 1706 | ||
Dehnung | -196.0 °C | 2.9 % Show Material materials with Dehnung of 2.9 % | F | DIN 1725-2, EN 1676, EN 1706 | |
-196.0 °C | 3.3 % Show Material materials with Dehnung of 3.3 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
-120.0 °C | 2.6 % Show Material materials with Dehnung of 2.6 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
-120.0 °C | 3.9 % Show Material materials with Dehnung of 3.9 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
-50.0 °C | 3.4 % Show Material materials with Dehnung of 3.4 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
-50.0 °C | 4.3 % Show Material materials with Dehnung of 4.3 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
3.0 % Show Material materials with Dehnung of 3.0 % | F | EN 1706 | A50 | ||
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 2.0 - 5.0 % Show Material materials with Dehnung of 2.0 - 5.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 2.0 - 4.0 % Show Material materials with Dehnung of 2.0 - 4.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 3.8 % Show Material materials with Dehnung of 3.8 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | F | EN 1706 | ||
20.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
Härte, Brinell | 60.0 [-] Show Material materials with Härte, Brinell of 60.0 [-] | F | EN 1706 | ||
65.0 [-] Show Material materials with Härte, Brinell of 65.0 [-] | F | EN 1706 | |||
20.0 °C | 55.0 [-] Show Material materials with Härte, Brinell of 55.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 60.0 [-] Show Material materials with Härte, Brinell of 60.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 60.0 - 75.0 [-] Show Material materials with Härte, Brinell of 60.0 - 75.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 65.0 - 85.0 [-] Show Material materials with Härte, Brinell of 65.0 - 85.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 5xx.x Series Aluminium | |||
Scherfestigkeit | 20.0 °C | 138.0 MPa Show Material materials with Scherfestigkeit of 138.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 150.0 MPa Show Material materials with Scherfestigkeit of 150.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
Zugfestigkeit | -196.0 °C | 198.0 MPa Show Material materials with Zugfestigkeit of 198.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | |
-196.0 °C | 219.0 MPa Show Material materials with Zugfestigkeit of 219.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
-120.0 °C | 175.0 MPa Show Material materials with Zugfestigkeit of 175.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
-120.0 °C | 203.0 MPa Show Material materials with Zugfestigkeit of 203.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
-50.0 °C | 172.0 MPa Show Material materials with Zugfestigkeit of 172.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
-50.0 °C | 187.0 MPa Show Material materials with Zugfestigkeit of 187.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
160.0 MPa Show Material materials with Zugfestigkeit of 160.0 MPa | F | EN 1706 | |||
180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | F | EN 1706 | |||
20.0 °C | 140.0 MPa Show Material materials with Zugfestigkeit of 140.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 150.0 MPa Show Material materials with Zugfestigkeit of 150.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 157.0 MPa Show Material materials with Zugfestigkeit of 157.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 160.0 - 200.0 MPa Show Material materials with Zugfestigkeit of 160.0 - 200.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 180.0 - 240.0 MPa Show Material materials with Zugfestigkeit of 180.0 - 240.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 184.0 MPa Show Material materials with Zugfestigkeit of 184.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | F | DIN 1725-2, EN 1676, EN 1706 |
100 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | F | DIN 1725-2, EN 1676, EN 1706 | |
200.0 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | F | DIN 1725-2, EN 1676, EN 1706 | |
Schmelzpunkt | 550.0 - 630.0 °C Show Material materials with Schmelzpunkt of 550.0 - 630.0 °C | F | EN 1706 | |
Spezifische Wärmekapazität | 930.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 930.0 J/(kg·K) | F | EN 1706 | |
20.0 °C | 930.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 930.0 J/(kg·K) | F | DIN 1725-2, EN 1676, EN 1706 | |
Wärmeleitfähigkeit | 110.0 - 140.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 110.0 - 140.0 W/(m·K) | F | EN 1706 | |
20.0 °C | 110.0 - 130.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 110.0 - 130.0 W/(m·K) | F | DIN 1725-2, EN 1676, EN 1706 |
Elektrisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Elektrische Leitfähigkeit | 15000000.0 - 21000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 15000000.0 - 21000000.0 S/m | F | EN 1706 | |
20.0 °C | 15000000.0 - 19000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 15000000.0 - 19000000.0 S/m | F | DIN 1725-2, EN 1676, EN 1706 | |
spezifischer Widerstand | 4.76e-08 - 6.67e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.76e-08 - 6.67e-08 Ω·m | F | EN 1706 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 91.6 % Show Material materials with Aluminium of 91.6 % | F | DIN 1725-2, EN 1676, EN 1706 |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
0.50 % Show Material materials with Eisen of 0.50 % | F | EN 1706 | |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | F | DIN 1725-2, EN 1676, EN 1706 |
Magnesium | 4.5 - 5.5 % Show Material materials with Magnesium of 4.5 - 5.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
Mangan | 0.001 - 0.4 % Show Material materials with Mangan of 0.001 - 0.4 % | F | DIN 1725-2, EN 1676, EN 1706 |
Silizium | 0.9 - 1.5 % Show Material materials with Silizium of 0.9 - 1.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
Titan | 0.001 - 0.2 % Show Material materials with Titan of 0.001 - 0.2 % | F | DIN 1725-2, EN 1676, EN 1706 |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | F | DIN 1725-2, EN 1676, EN 1706 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good | |
Corrosion properties | general: excellent | |
General machinability | after thermal treatment: excellent | |
Processing methods | permanent mould casting |