Allgemein
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 - 90.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa | F | EN 1706 | ||
Dehnung | 1.0 % Show Material materials with Dehnung of 1.0 % | F | EN 1706 | A50 | |
20.0 °C | 1.0 - 3.0 % Show Material materials with Dehnung of 1.0 - 3.0 % | F | DIN 1725-2, EN 1676, EN 1706 | ||
Elastizitätsmodul | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | F | EN 1706 | ||
20.0 °C | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | F | DIN 1725-2, EN 1676, EN 1706 | ||
Härte, Brinell | 70.0 [-] Show Material materials with Härte, Brinell of 70.0 [-] | F | EN 1706 | ||
20.0 °C | 70.0 - 100.0 [-] Show Material materials with Härte, Brinell of 70.0 - 100.0 [-] | F | DIN 1725-2, EN 1676, EN 1706 | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 5xx.x Series Aluminium | |||
Zugfestigkeit | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | F | EN 1706 | ||
20.0 °C | 200.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 200.0 - 300.0 MPa | F | DIN 1725-2, EN 1676, EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | F | EN 1706 |
20 °C | 2.4999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K | F | EN 1706 | |
100 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | F | EN 1706 | |
200 °C | 2.4999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K | F | EN 1706 | |
200.0 °C | 2.5e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5e-05 1/K | F | DIN 1725-2, EN 1676, EN 1706 | |
Schmelzpunkt | 530.0 - 620.0 °C Show Material materials with Schmelzpunkt of 530.0 - 620.0 °C | F | EN 1706 | |
Spezifische Wärmekapazität | 940.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 940.0 J/(kg·K) | F | EN 1706 | |
20.0 °C | 940.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 940.0 J/(kg·K) | F | DIN 1725-2, EN 1676, EN 1706 | |
Wärmeleitfähigkeit | 60.0 - 90.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 60.0 - 90.0 W/(m·K) | F | EN 1706 | |
20.0 °C | 80.0 - 100.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 80.0 - 100.0 W/(m·K) | F | DIN 1725-2, EN 1676, EN 1706 |
Elektrisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Elektrische Leitfähigkeit | 11000000.0 - 14000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 11000000.0 - 14000000.0 S/m | F | EN 1706 | |
20.0 °C | 12000000.0 - 15000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 12000000.0 - 15000000.0 S/m | F | DIN 1725-2, EN 1676, EN 1706 | |
spezifischer Widerstand | 7.14e-08 - 9.09e-08 Ω·m Show Material materials with spezifischer Widerstand of 7.14e-08 - 9.09e-08 Ω·m | F | EN 1706 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 85.6 % Show Material materials with Aluminium of 85.6 % | F | DIN 1725-2, EN 1676, EN 1706 |
Eisen | 1.0 % Show Material materials with Eisen of 1.0 % | F | DIN 1725-2, EN 1676, EN 1706 |
1.00 % Show Material materials with Eisen of 1.00 % | F | EN 1706 | |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | F | DIN 1725-2, EN 1676, EN 1706 |
Magnesium | 7.0 - 10.0 % Show Material materials with Magnesium of 7.0 - 10.0 % | F | DIN 1725-2, EN 1676, EN 1706 |
Mangan | 0.2 - 0.5 % Show Material materials with Mangan of 0.2 - 0.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
0.5 % Show Material materials with Mangan of 0.5 % | F | EN 1706 | |
Silizium | 0.01 - 2.5 % Show Material materials with Silizium of 0.01 - 2.5 % | F | DIN 1725-2, EN 1676, EN 1706 |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | F | DIN 1725-2, EN 1676, EN 1706 |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | F | DIN 1725-2, EN 1676, EN 1706 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good | |
Corrosion properties | general: excellent | |
General machinability | after thermal treatment: excellent | |
Processing methods | pressure die casting, separately cast test sample |