Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.4 - 8.41 g/cm³ Show Material materials with Dichte of 8.4 - 8.41 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 20 - 23 % Show Material materials with Dehnung of 20 - 23 % |
Dehnung A50 | 20.0 °C | 15 % Show Material materials with Dehnung A50 of 15 % |
Dehnung, transversal | 20.0 °C | 23 % Show Material materials with Dehnung, transversal of 23 % |
Elastizitätsmodul | -195.0 °C | 108 GPa Show Material materials with Elastizitätsmodul of 108 GPa |
-100.0 °C | 106 GPa Show Material materials with Elastizitätsmodul of 106 GPa | |
20.0 °C | 102 - 105 GPa Show Material materials with Elastizitätsmodul of 102 - 105 GPa | |
50.0 °C | 100 GPa Show Material materials with Elastizitätsmodul of 100 GPa | |
100.0 °C | 93 - 99 GPa Show Material materials with Elastizitätsmodul of 93 - 99 GPa | |
150.0 °C | 91 GPa Show Material materials with Elastizitätsmodul of 91 GPa | |
200.0 °C | 89 - 94 GPa Show Material materials with Elastizitätsmodul of 89 - 94 GPa | |
250.0 °C | 83 GPa Show Material materials with Elastizitätsmodul of 83 GPa | |
300.0 °C | 89 GPa Show Material materials with Elastizitätsmodul of 89 GPa | |
400.0 °C | 83 GPa Show Material materials with Elastizitätsmodul of 83 GPa | |
500.0 °C | 74 GPa Show Material materials with Elastizitätsmodul of 74 GPa | |
600.0 °C | 64 GPa Show Material materials with Elastizitätsmodul of 64 GPa | |
700.0 °C | 54 GPa Show Material materials with Elastizitätsmodul of 54 GPa | |
Poissonzahl | 20.0 °C | 0.34 [-] Show Material materials with Poissonzahl of 0.34 [-] |
Schubmodule | 20.0 °C | 37 GPa Show Material materials with Schubmodule of 37 GPa |
Streckgrenze Rp 0,2 | 20.0 °C | 190 - 250 MPa Show Material materials with Streckgrenze Rp 0,2 of 190 - 250 MPa |
50.0 °C | 250 MPa Show Material materials with Streckgrenze Rp 0,2 of 250 MPa | |
100.0 °C | 225 MPa Show Material materials with Streckgrenze Rp 0,2 of 225 MPa | |
150.0 °C | 200 MPa Show Material materials with Streckgrenze Rp 0,2 of 200 MPa | |
Streckgrenze Rp 0,2, transversal | 20.0 °C | 240 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 240 MPa |
50.0 °C | 240 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 240 MPa | |
100.0 °C | 220 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 220 MPa | |
150.0 °C | 200 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 200 MPa | |
Zugfestigkeit | 20.0 °C | 400 - 480 MPa Show Material materials with Zugfestigkeit of 400 - 480 MPa |
Zugfestigkeit, transversal | 20.0 °C | 400 MPa Show Material materials with Zugfestigkeit, transversal of 400 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.7E-5 - 2.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 - 2.1E-5 1/K | Typical for Wrought Copper Brass |
Schmelzpunkt | 875 - 1075 °C Show Material materials with Schmelzpunkt of 875 - 1075 °C | Typical for Wrought Copper Brass | |
Spezifische Wärmekapazität | 20.0 °C | 375 - 377 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 375 - 377 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 109 - 117 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 109 - 117 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 1.39E+7 - 1.50E+7 S/m Show Material materials with Elektrische Leitfähigkeit of 1.39E+7 - 1.50E+7 S/m |
Specific Electrical conductivity | 24 - 26 % IACS Show Material materials with Specific Electrical conductivity of 24 - 26 % IACS | |
spezifischer Widerstand | 20.0 °C | 6.7E-8 Ω·m Show Material materials with spezifischer Widerstand of 6.7E-8 Ω·m |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.05 % Show Material materials with Aluminium of 0.05 % |
Blei | 0.2 - 0.3 % Show Material materials with Blei of 0.2 - 0.3 % |
Eisen | 0.2 % Show Material materials with Eisen of 0.2 % |
Kupfer | 59 - 61.5 % Show Material materials with Kupfer of 59 - 61.5 % |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % |
Zinn | 0.2 % Show Material materials with Zinn of 0.2 % |