Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.8 g/cm³ Show Material materials with Dichte of 8.8 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 20 - 25 % Show Material materials with Dehnung of 20 - 25 % | |
Elastizitätsmodul | 23.0 °C | 110 - 130 GPa Show Material materials with Elastizitätsmodul of 110 - 130 GPa | Typical for Wrought Copper High Copper Alloy |
Elongation A10 | 20.0 °C | 18 - 22 % Show Material materials with Elongation A10 of 18 - 22 % | |
Elongation A100 | 20.0 °C | 15 - 20 % Show Material materials with Elongation A100 of 15 - 20 % | |
Härte, Brinell | 20.0 °C | 65 - 95 [-] Show Material materials with Härte, Brinell of 65 - 95 [-] | |
Härte, Vickers | 20.0 °C | 70 - 100 [-] Show Material materials with Härte, Vickers of 70 - 100 [-] | |
Streckgrenze Rp 0,2 | 20.0 °C | 135 - 200 MPa Show Material materials with Streckgrenze Rp 0,2 of 135 - 200 MPa | |
Zugfestigkeit | 20.0 °C | 240 - 380 MPa Show Material materials with Zugfestigkeit of 240 - 380 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.6E-5 - 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 - 1.8E-5 1/K | Typical for Wrought Copper High Copper Alloy |
Max. Betriebstemperatur, lang | 0 - 350 °C Show Material materials with Max. Betriebstemperatur, lang of 0 - 350 °C | ||
Schmelzpunkt | 855 - 1090 °C Show Material materials with Schmelzpunkt of 855 - 1090 °C | Typical for Wrought Copper High Copper Alloy | |
Spezifische Wärmekapazität | 23.0 °C | 360 - 420 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 360 - 420 J/(kg·K) | Typical for Wrought Copper High Copper Alloy |
Chemical properties
Property | Value |
---|---|
Beryllium | 0.4 - 0.7 % Show Material materials with Beryllium of 0.4 - 0.7 % |
Eisen | 0.2 % Show Material materials with Eisen of 0.2 % |
Kobalt | 2 - 2.8 % Show Material materials with Kobalt of 2 - 2.8 % |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % |