Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.5 g/cm³ Show Material materials with Dichte of 8.5 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 27 % Show Material materials with Dehnung of 27 % |
Elastizitätsmodul | 20.0 °C | 112 GPa Show Material materials with Elastizitätsmodul of 112 GPa |
Elongation A10 | 20.0 °C | 24 % Show Material materials with Elongation A10 of 24 % |
Elongation A100 | 20.0 °C | 20 % Show Material materials with Elongation A100 of 20 % |
Poissonzahl | 20.0 °C | 0.34 [-] Show Material materials with Poissonzahl of 0.34 [-] |
Schubmodule | 20.0 °C | 40 GPa Show Material materials with Schubmodule of 40 GPa |
Streckgrenze Rp 0,2 | 20.0 °C | 120 MPa Show Material materials with Streckgrenze Rp 0,2 of 120 MPa |
Zugfestigkeit | 20.0 °C | 310 MPa Show Material materials with Zugfestigkeit of 310 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.7E-5 - 2.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 - 2.1E-5 1/K | Typical for Wrought Copper Brass |
Schmelzpunkt | 875 - 1075 °C Show Material materials with Schmelzpunkt of 875 - 1075 °C | Typical for Wrought Copper Brass | |
Spezifische Wärmekapazität | 20.0 °C | 377 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 377 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 121 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 121 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 1.55E+7 - 1.60E+7 S/m Show Material materials with Elektrische Leitfähigkeit of 1.55E+7 - 1.60E+7 S/m |
Specific Electrical conductivity | 28 % IACS Show Material materials with Specific Electrical conductivity of 28 % IACS | |
spezifischer Widerstand | 20.0 °C | 6.5E-8 Ω·m Show Material materials with spezifischer Widerstand of 6.5E-8 Ω·m |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % |
Blei | 0.05 % Show Material materials with Blei of 0.05 % |
Eisen | 0.05 % Show Material materials with Eisen of 0.05 % |
Kupfer | 66 - 68.5 % Show Material materials with Kupfer of 66 - 68.5 % |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % |
Zinn | 0.1 % Show Material materials with Zinn of 0.1 % |