EN 12167 Grade CuNi2Be R680

View suppliers (2)
Want to keep this datasheet? Save it now in your required format

Description

CuNi2Be, mat. No CW110C, is counted among hardenable, low alloyed copper alloys. To the comparable make CuNi2Be, mat. No 2.0850, acc. to DIN 17666 : 1983-12 applies: The alloy shows high tensile strength and high temperature resistance and mean electrical and favorable thermal conductivity. Processing properties: hot and cold forming: good machinability: moderately hard and soft soldering: good gas shielded welding: good burnishing: good Application: For resistance welding electrodes as well as for springs. For the electrolytically tinned strip the coatings (Sn bright, Sn matt, Sn fuzed, SnPb) are listed by the application (better solderability, better corrosion resistance, reduction of the electrical contact resistance, better appearance) in the DIN EN 14436 : 2004-11 (Table 5)

Related Standards

Equivalent Materials

Diese Materialdaten wurden von WIAM zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Eigenschaften

Allgemein

PropertyTemperatureValue

Dichte

20.0 °C

8.8 g/cm³

Show Material materials with Dichte of 8.8 g/cm³

Mechanisch

PropertyTemperatureValueComment

Dehnung

20.0 °C

8 %

Show Material materials with Dehnung of 8 %

Elastizitätsmodul

23.0 °C

110 - 130 GPa

Show Material materials with Elastizitätsmodul of 110 - 130 GPa

Typical for Wrought Copper High Copper Alloy

Elongation A100

20.0 °C

4 %

Show Material materials with Elongation A100 of 4 %

Elongation A11.3

20.0 °C

6 %

Show Material materials with Elongation A11.3 of 6 %

Streckgrenze Rp 0,2

20.0 °C

540 MPa

Show Material materials with Streckgrenze Rp 0,2 of 540 MPa

Zugfestigkeit

20.0 °C

680 MPa

Show Material materials with Zugfestigkeit of 680 MPa

Thermisch

PropertyTemperatureValueComment

Koeffizient der thermischen Ausdehnung

23.0 °C

1.6E-5 - 1.8E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 - 1.8E-5 1/K

Typical for Wrought Copper High Copper Alloy

Schmelzpunkt

855 - 1090 °C

Show Material materials with Schmelzpunkt of 855 - 1090 °C

Typical for Wrought Copper High Copper Alloy

Spezifische Wärmekapazität

23.0 °C

360 - 420 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 360 - 420 J/(kg·K)

Typical for Wrought Copper High Copper Alloy

Elektrisch

PropertyTemperatureValue

Elektrische Leitfähigkeit

20.0 °C

3.80E+7 S/m

Show Material materials with Elektrische Leitfähigkeit of 3.80E+7 S/m

Specific Electrical conductivity

65 % IACS

Show Material materials with Specific Electrical conductivity of 65 % IACS

Chemical properties

PropertyValue

Beryllium

0.2 - 0.6 %

Show Material materials with Beryllium of 0.2 - 0.6 %

Eisen

0.2 %

Show Material materials with Eisen of 0.2 %

Kobalt

0.3 %

Show Material materials with Kobalt of 0.3 %

Nickel

1.4 - 2.4 %

Show Material materials with Nickel of 1.4 - 2.4 %