CuSn8, mat. No. CW453K, is comparable to the DIN-make CuSn8, mat. No. 2.1030, acc. to DIN 17662 : 1983-12. Properties of the CuSn-alloy are predominantly determined by the tin-content. Tensile strength, yield point and hardness increase according to the rising cold forming grade, elongation after fracture decreases. Electrical and thermal conductivity are lower than for pure copper. Very high resistance to corrosion, particularly to atmospheric influences, seawater, sulfite liquor, carbonated and salted mine water. The alloys are stress corrosion-proof. Processing properties: warm forming: medium cold forming: very good machinability: medium hard soldering: good soft soldering: good gas shielded welding: good burnishing: good Application: For friction elements, especially for thin-walled friction-bearing bushings and sliding strips as well as for beater bars. Increased abrasion and corrosion resistance compared to CuSn6. For the electrolytically tinned strip the coatings (Sn bright, Sn matt, Sn fuzed, SnPb) are listed by the application (better solderability, better corrosion resistance, reduction of the electrical contact resistance, better appearance) in the DIN EN 14436 : 2004-11 (Table 5)

Related Standards

Equivalent Materials

Diese Materialdaten wurden von WIAM zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Eigenschaften

Allgemein

PropertyTemperatureValue

Dichte

20.0 °C

8.79 - 8.8 g/cm³

Show Material materials with Dichte of 8.79 - 8.8 g/cm³

Mechanisch

PropertyTemperatureValue

Dehnung

20.0 °C

23 - 26 %

Show Material materials with Dehnung of 23 - 26 %

Dehnung A50

20.0 °C

20 - 23 %

Show Material materials with Dehnung A50 of 20 - 23 %

Elastizitätsmodul

20.0 °C

115 GPa

Show Material materials with Elastizitätsmodul of 115 GPa

Elongation A10

20.0 °C

22 %

Show Material materials with Elongation A10 of 22 %

Elongation A100

20.0 °C

18 %

Show Material materials with Elongation A100 of 18 %

Elongation A11.3

20.0 °C

22 %

Show Material materials with Elongation A11.3 of 22 %

Poissonzahl

20.0 °C

0.34 [-]

Show Material materials with Poissonzahl of 0.34 [-]

Streckgrenze Rp 0,2

20.0 °C

250 - 280 MPa

Show Material materials with Streckgrenze Rp 0,2 of 250 - 280 MPa

Zugfestigkeit

20.0 °C

450 - 550 MPa

Show Material materials with Zugfestigkeit of 450 - 550 MPa

Thermisch

PropertyTemperatureValue

Koeffizient der thermischen Ausdehnung

100.0 °C

1.8E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K

300.0 °C

1.82E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.82E-5 1/K

400.0 °C

1.87E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 1.87E-5 1/K

650.0 °C

2.22E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.22E-5 1/K

800.0 °C

2.18E-5 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.18E-5 1/K

Spezifische Wärmekapazität

20.0 °C

377 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 377 J/(kg·K)

Wärmeleitfähigkeit

20.0 °C

67 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 67 W/(m·K)

200.0 °C

81 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 81 W/(m·K)

Unlock all property charts

Elektrisch

PropertyTemperatureValue

Elektrische Leitfähigkeit

20.0 °C

7.00E+6 - 7.50E+6 S/m

Show Material materials with Elektrische Leitfähigkeit of 7.00E+6 - 7.50E+6 S/m

200.0 °C

6.50E+6 S/m

Show Material materials with Elektrische Leitfähigkeit of 6.50E+6 S/m

Unlock all property charts

Specific Electrical conductivity

12 - 13 % IACS

Show Material materials with Specific Electrical conductivity of 12 - 13 % IACS

spezifischer Widerstand

20.0 °C

1.33E-7 Ω·m

Show Material materials with spezifischer Widerstand of 1.33E-7 Ω·m

200.0 °C

1.54E-7 Ω·m

Show Material materials with spezifischer Widerstand of 1.54E-7 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Blei

0.02 %

Show Material materials with Blei of 0.02 %

Eisen

0.1 %

Show Material materials with Eisen of 0.1 %

Nickel

0.2 %

Show Material materials with Nickel of 0.2 %

Phosphor

0.01 - 0.4 %

Show Material materials with Phosphor of 0.01 - 0.4 %

Zink

0.2 %

Show Material materials with Zink of 0.2 %

Zinn

7.5 - 8.5 %