Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.78 g/cm³ Show Material materials with Dichte of 2.78 g/cm³ | T3511 | AA Standards, ASTM B241 | |
2.79 g/cm³ Show Material materials with Dichte of 2.79 g/cm³ | T3511 | Bar, Tube | ||
3.0 g/cm³ Show Material materials with Dichte of 3.0 g/cm³ | T3511 |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Dehnung | 7.0 % Show Material materials with Dehnung of 7.0 % | T3511 | AA Standards, ASTM B241 | A100 | |
8.8 % Show Material materials with Dehnung of 8.8 % | T3511 | ||||
9.0 % Show Material materials with Dehnung of 9.0 % | T3511 | AA Standards, ASTM B241 | A100 | ||
10.0 % Show Material materials with Dehnung of 10.0 % | T3511 | AA Standards, ASTM B241 | A50 | ||
10.0 - 12.0 % Show Material materials with Dehnung of 10.0 - 12.0 % | T3511 | Bar, Tube | |||
Elastizitätsmodul | 73.0 GPa Show Material materials with Elastizitätsmodul of 73.0 GPa | T3511 | AA Standards, ASTM B241 | Bar, Tube | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | |||
Schubmodule | 26.0 - 27.5 GPa Show Material materials with Schubmodule of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | |||
Streckgrenze | 290.0 MPa Show Material materials with Streckgrenze of 290.0 MPa | T3511 | AA Standards, ASTM B241 | RP02 | |
290.0 - 358.0 MPa Show Material materials with Streckgrenze of 290.0 - 358.0 MPa | T3511 | Bar, Tube | RP02 | ||
305.0 MPa Show Material materials with Streckgrenze of 305.0 MPa | T3511 | AA Standards, ASTM B241 | RP02 | ||
315.0 MPa Show Material materials with Streckgrenze of 315.0 MPa | T3511 | AA Standards, ASTM B241 | RP02 | ||
330.0 MPa Show Material materials with Streckgrenze of 330.0 MPa | T3511 | AA Standards, ASTM B241 | RP02 | ||
330.0 MPa Show Material materials with Streckgrenze of 330.0 MPa | T3511 | ||||
Zugfestigkeit | 392.0 - 482.0 MPa Show Material materials with Zugfestigkeit of 392.0 - 482.0 MPa | T3511 | Bar, Tube | ||
395.0 MPa Show Material materials with Zugfestigkeit of 395.0 MPa | T3511 | AA Standards, ASTM B241 | |||
415.0 MPa Show Material materials with Zugfestigkeit of 415.0 MPa | T3511 | AA Standards, ASTM B241 | |||
450.0 MPa Show Material materials with Zugfestigkeit of 450.0 MPa | T3511 | AA Standards, ASTM B241 | |||
470.0 MPa Show Material materials with Zugfestigkeit of 470.0 MPa | T3511 | AA Standards, ASTM B241 |
Thermisch
Property | Temperature | Value | Condition | Shape | Related Standards |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T3511 | |||
2.31e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.31e-05 1/K | T3511 | Bar, Tube | |||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | T3511 | AA Standards, ASTM B241 | ||
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | T3511 | AA Standards, ASTM B241 | ||
Schmelzpunkt | 500.0 °C Show Material materials with Schmelzpunkt of 500.0 °C | T3511 | |||
505.0 - 635.0 °C Show Material materials with Schmelzpunkt of 505.0 - 635.0 °C | T3511 | AA Standards, ASTM B241 | |||
640.0 °C Show Material materials with Schmelzpunkt of 640.0 °C | T3511 | Bar, Tube | |||
Spezifische Wärmekapazität | 870.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 870.0 J/(kg·K) | T3511 | |||
Wärmeleitfähigkeit | 120.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 120.0 W/(m·K) | T3511 | |||
121.0 - 193.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 121.0 - 193.0 W/(m·K) | T3511 | AA Standards, ASTM B241 | |||
121.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 121.0 - 150.0 W/(m·K) | T3511 | Bar, Tube |
Elektrisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Elektrische Leitfähigkeit | 17000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 17000000.0 - 29000000.0 S/m | T3511 | AA Standards, ASTM B241 | |
spezifischer Widerstand | 3.45e-08 - 5.88e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.45e-08 - 5.88e-08 Ω·m | T3511 | AA Standards, ASTM B241 | |
4.31e-08 - 5.75e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.31e-08 - 5.75e-08 Ω·m | T3511 | Bar, Tube |
Chemical properties
Property | Value | Condition | Shape | Related Standards | Comment |
---|---|---|---|---|---|
Aluminium | 90.7 - 94.7 % Show Material materials with Aluminium of 90.7 - 94.7 % | T3511 | |||
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T3511 | Bar, Tube | Total | |
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | T3511 | Bar, Tube | AA Standards, ASTM B241 | |
Eisen | 0.50 % Show Material materials with Eisen of 0.50 % | T3511 | AA Standards, ASTM B241 | ||
0.5 % Show Material materials with Eisen of 0.5 % | T3511 | Bar, Tube | |||
Kupfer | 3.8 - 4.9 % Show Material materials with Kupfer of 3.8 - 4.9 % | T3511 | Bar, Tube | AA Standards, ASTM B241 | |
Magnesium | 1.2 - 1.8 % Show Material materials with Magnesium of 1.2 - 1.8 % | T3511 | Bar, Tube | AA Standards, ASTM B241 | |
Mangan | 0.3 - 0.9 % Show Material materials with Mangan of 0.3 - 0.9 % | T3511 | Bar, Tube | AA Standards, ASTM B241 | |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | T3511 | Bar, Tube | AA Standards, ASTM B241 | |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | T3511 | Bar, Tube | AA Standards, ASTM B241 | |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | T3511 | Bar, Tube | AA Standards, ASTM B241 | |
Zirkonium | 0.2 % Show Material materials with Zirkonium of 0.2 % | T3511 |
Technological properties
Property | ||
---|---|---|
Application areas | Aerospace, High strength applications | |
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Betriebsschäden in Gebieten mit Zugspannungen quer zur Kornstruktur, Eingeschränkte Schäden an Laborproben (T4,T3, T351, T3510, T3511), d (T6, T861, T81, T851, T8510, T8511), general: sufficient, in principle it should be protected | |
General machinability | General: poor (O), good to acceptable | |
Workability | general (condition): poor(T4, T3, T351, T3510, T3511, T6), not suitable (T361, T861, T81, T851, T8510, T8511) |