Allgemein
Property | Value | Condition |
---|---|---|
Dichte | 3.1 g/cm³ Show Material materials with Dichte of 3.1 g/cm³ | T3 |
Mechanisch
Property | Value | Condition | Comment |
---|---|---|---|
Dehnung | 13.0 % Show Material materials with Dehnung of 13.0 % | T3 | |
Elastizitätsmodul | 74.0 GPa Show Material materials with Elastizitätsmodul of 74.0 GPa | T3 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | |
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | |
Schubmodule | 26.0 - 27.5 GPa Show Material materials with Schubmodule of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | |
Streckgrenze | 220.0 MPa Show Material materials with Streckgrenze of 220.0 MPa | T3 | |
Zugfestigkeit | 330.0 MPa Show Material materials with Zugfestigkeit of 330.0 MPa | T3 |
Thermisch
Property | Value | Condition |
---|---|---|
Koeffizient der thermischen Ausdehnung | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T3 |
Schmelzpunkt | 540.0 °C Show Material materials with Schmelzpunkt of 540.0 °C | T3 |
Spezifische Wärmekapazität | 860.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 860.0 J/(kg·K) | T3 |
Wärmeleitfähigkeit | 110.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 110.0 W/(m·K) | T3 |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 30000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 30000000.0 S/m | Typical for Wrought 2000 Series Aluminium |
spezifischer Widerstand | 3.4e-08 - 6e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 6e-08 Ω·m | Typical for Wrought 2000 Series Aluminium |
Chemical properties
Property | Value | Condition |
---|---|---|
Aluminium | 91.5 - 93.8 % Show Material materials with Aluminium of 91.5 - 93.8 % | T3 |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T3 |
Eisen | 0.3 % Show Material materials with Eisen of 0.3 % | T3 |
Kupfer | 5.8 - 6.8 % Show Material materials with Kupfer of 5.8 - 6.8 % | T3 |
Magnesium | 0.02 % Show Material materials with Magnesium of 0.02 % | T3 |
Mangan | 0.2 - 0.4 % Show Material materials with Mangan of 0.2 - 0.4 % | T3 |
Silizium | 0.2 % Show Material materials with Silizium of 0.2 % | T3 |
Titan | 0.02 - 0.1 % Show Material materials with Titan of 0.02 - 0.1 % | T3 |
Vanadium | 0.05 - 0.15 % Show Material materials with Vanadium of 0.05 - 0.15 % | T3 |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | T3 |
Zirkonium | 0.1 - 0.25 % Show Material materials with Zirkonium of 0.1 - 0.25 % | T3 |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |