Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.84 g/cm³ Show Material materials with Dichte of 2.84 g/cm³ | T37 | AA Standards, ASTM B209 |
3.1 g/cm³ Show Material materials with Dichte of 3.1 g/cm³ | T37 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Dehnung | 3.0 % Show Material materials with Dehnung of 3.0 % | T37 | AA Standards, ASTM B209 | A100 |
4.0 % Show Material materials with Dehnung of 4.0 % | T37 | AA Standards, ASTM B209 | A100 | |
5.0 % Show Material materials with Dehnung of 5.0 % | T37 | AA Standards, ASTM B209 | A100 | |
6.0 % Show Material materials with Dehnung of 6.0 % | T37 | AA Standards, ASTM B209 | A50 | |
8.5 % Show Material materials with Dehnung of 8.5 % | T37 | |||
Elastizitätsmodul | 73.0 GPa Show Material materials with Elastizitätsmodul of 73.0 GPa | T37 | AA Standards, ASTM B209 | |
74.0 GPa Show Material materials with Elastizitätsmodul of 74.0 GPa | T37 | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||
Schubmodule | 26.0 - 27.5 GPa Show Material materials with Schubmodule of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | ||
Streckgrenze | 235.0 MPa Show Material materials with Streckgrenze of 235.0 MPa | T37 | AA Standards, ASTM B209 | RP02 |
240.0 MPa Show Material materials with Streckgrenze of 240.0 MPa | T37 | AA Standards, ASTM B209 | RP02 | |
250.0 MPa Show Material materials with Streckgrenze of 250.0 MPa | T37 | AA Standards, ASTM B209 | RP02 | |
255.0 MPa Show Material materials with Streckgrenze of 255.0 MPa | T37 | AA Standards, ASTM B209 | RP02 | |
260.0 MPa Show Material materials with Streckgrenze of 260.0 MPa | T37 | AA Standards, ASTM B209 | RP02 | |
300.0 MPa Show Material materials with Streckgrenze of 300.0 MPa | T37 | |||
Zugfestigkeit | 295.0 MPa Show Material materials with Zugfestigkeit of 295.0 MPa | T37 | AA Standards, ASTM B209 | |
310.0 MPa Show Material materials with Zugfestigkeit of 310.0 MPa | T37 | AA Standards, ASTM B209 | ||
325.0 MPa Show Material materials with Zugfestigkeit of 325.0 MPa | T37 | AA Standards, ASTM B209 | ||
340.0 MPa Show Material materials with Zugfestigkeit of 340.0 MPa | T37 | AA Standards, ASTM B209 | ||
380.0 MPa Show Material materials with Zugfestigkeit of 380.0 MPa | T37 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T37 | ||
20 °C | 2.23e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K | T37 | AA Standards, ASTM B209 | |
100 °C | 2.23e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K | T37 | AA Standards, ASTM B209 | |
Schmelzpunkt | 540.0 °C Show Material materials with Schmelzpunkt of 540.0 °C | T37 | ||
545.0 - 645.0 °C Show Material materials with Schmelzpunkt of 545.0 - 645.0 °C | T37 | AA Standards, ASTM B209 | ||
Spezifische Wärmekapazität | 860.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 860.0 J/(kg·K) | T37 | ||
Wärmeleitfähigkeit | 110.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 110.0 W/(m·K) | T37 | ||
113.0 - 172.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 113.0 - 172.0 W/(m·K) | T37 | AA Standards, ASTM B209 |
Elektrisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Elektrische Leitfähigkeit | 16000000.0 - 26000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 16000000.0 - 26000000.0 S/m | T37 | AA Standards, ASTM B209 | |
16000000 S/m Show Material materials with Elektrische Leitfähigkeit of 16000000 S/m | T37 | Typical/derived value | ||
Specific Electrical conductivity | 28.0 % IACS Show Material materials with Specific Electrical conductivity of 28.0 % IACS | T37 | Typical value | |
spezifischer Widerstand | 3.85e-08 - 6.25e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.85e-08 - 6.25e-08 Ω·m | T37 | AA Standards, ASTM B209 | |
6.15e-08 Ω·m Show Material materials with spezifischer Widerstand of 6.15e-08 Ω·m | T37 | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 91.5 - 93.8 % Show Material materials with Aluminium of 91.5 - 93.8 % | T37 | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T37 | |
Eisen | 0.30 % Show Material materials with Eisen of 0.30 % | T37 | AA Standards, ASTM B209 |
0.3 % Show Material materials with Eisen of 0.3 % | T37 | ||
Kupfer | 5.8 - 6.8 % Show Material materials with Kupfer of 5.8 - 6.8 % | T37 | AA Standards, ASTM B209 |
Magnesium | 0.02 % Show Material materials with Magnesium of 0.02 % | T37 | AA Standards, ASTM B209 |
Mangan | 0.2 - 0.4 % Show Material materials with Mangan of 0.2 - 0.4 % | T37 | AA Standards, ASTM B209 |
Silizium | 0.2 % Show Material materials with Silizium of 0.2 % | T37 | AA Standards, ASTM B209 |
Titan | 0.02 - 0.1 % Show Material materials with Titan of 0.02 - 0.1 % | T37 | AA Standards, ASTM B209 |
Vanadium | 0.05 - 0.15 % Show Material materials with Vanadium of 0.05 - 0.15 % | T37 | AA Standards, ASTM B209 |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | T37 | AA Standards, ASTM B209 |
Zirkonium | 0.1 - 0.25 % Show Material materials with Zirkonium of 0.1 - 0.25 % | T37 | AA Standards, ASTM B209 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Betriebsschäden in Gebieten mit Zugspannungen quer zur Kornstruktur, Eingeschränkte Schäden an Laborproben (T31, T351, T3510, T3511, T37), kein Schadensfall im Betrieb, eingeschränkte Schäden bei den Labortests (T81, T851, T8510, T8511), general: sufficient, in principle it should be protected | |
General machinability | General: good to acceptable | |
Workability | general (condition): poor(T31, T351, T3510, T3511), not suitable (T37, T81, T851, T8510, T8511, T87) |