Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.84 g/cm³ Show Material materials with Dichte of 2.84 g/cm³ | T87 | AA Standards, ASTM B209 |
2.84 g/cm³ Show Material materials with Dichte of 2.84 g/cm³ | T87 | ||
3.1 g/cm³ Show Material materials with Dichte of 3.1 g/cm³ | T87 |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 105.0 MPa Show Material materials with Bending Fatigue Strength of 105.0 MPa | T87 | AA Standards | ||
Dauerfestigkeit | 103 MPa Show Material materials with Dauerfestigkeit of 103 MPa | T87 | for 5x10⁸ cycles | ||
Dehnung | 2.0 % Show Material materials with Dehnung of 2.0 % | T87 | AA Standards, ASTM B209 | A100 | |
3.0 % Show Material materials with Dehnung of 3.0 % | T87 | AA Standards, ASTM B209 | A100 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | T87 | AA Standards, ASTM B209 | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | T87 | AA Standards, ASTM B209 | A100 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | T87 | AA Standards, ASTM B209 | A50 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | T87 | AA Standards, ASTM B209 | A100 | ||
7.0 % Show Material materials with Dehnung of 7.0 % | T87 | AA Standards, ASTM B209 | A50 | ||
7.4 % Show Material materials with Dehnung of 7.4 % | T87 | ||||
10.0 % Show Material materials with Dehnung of 10.0 % | T87 | AA Standards | A50 | ||
10 % Show Material materials with Dehnung of 10 % | T87 | ||||
Elastizitätsmodul | 73.0 GPa Show Material materials with Elastizitätsmodul of 73.0 GPa | T87 | AA Standards, ASTM B209 | ||
73 GPa Show Material materials with Elastizitätsmodul of 73 GPa | T87 | ||||
74.0 GPa Show Material materials with Elastizitätsmodul of 74.0 GPa | T87 | ||||
Kriechfestigkeit | 24 °C | 420 MPa Show Material materials with Kriechfestigkeit of 420 MPa | T87 | up to 1000 hours | |
100 °C | 315 MPa Show Material materials with Kriechfestigkeit of 315 MPa | T87 | up to 1000 hours | ||
150 °C | 235 MPa Show Material materials with Kriechfestigkeit of 235 MPa | T87 | up to 1000 hours | ||
205 °C | 150 MPa Show Material materials with Kriechfestigkeit of 150 MPa | T87 | up to 1000 hours | ||
230 °C | 130 MPa Show Material materials with Kriechfestigkeit of 130 MPa | T87 | up to 1000 hours | ||
260 °C | 105 MPa Show Material materials with Kriechfestigkeit of 105 MPa | T87 | up to 1000 hours | ||
270 °C | 17 MPa Show Material materials with Kriechfestigkeit of 17 MPa | T87 | up to 1000 hours | ||
315 °C | 34 MPa Show Material materials with Kriechfestigkeit of 34 MPa | T87 | up to 1000 hours | ||
Plane-Strain Fracture Toughnes | -196 °C | 38.9 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 38.9 MPa·√m | T87 | For plate in T-L direction | |
24 °C | 30.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.8 MPa·√m | T87 | For plate in T-L direction | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | |||
Schubmodule | 26.0 GPa Show Material materials with Schubmodule of 26.0 GPa | T87 | |||
Streckgrenze | 340.0 MPa Show Material materials with Streckgrenze of 340.0 MPa | T87 | AA Standards, ASTM B209 | RP02 | |
345.0 MPa Show Material materials with Streckgrenze of 345.0 MPa | T87 | AA Standards, ASTM B209 | RP02 | ||
350.0 MPa Show Material materials with Streckgrenze of 350.0 MPa | T87 | AA Standards, ASTM B209 | RP02 | ||
360.0 MPa Show Material materials with Streckgrenze of 360.0 MPa | T87 | AA Standards, ASTM B209 | RP02 | ||
395.0 MPa Show Material materials with Streckgrenze of 395.0 MPa | T87 | AA Standards | RP02 | ||
395 MPa Show Material materials with Streckgrenze of 395 MPa | T87 | RP02 | |||
400.0 MPa Show Material materials with Streckgrenze of 400.0 MPa | T87 | ||||
Zugfestigkeit | 420.0 MPa Show Material materials with Zugfestigkeit of 420.0 MPa | T87 | AA Standards, ASTM B209 | ||
425.0 MPa Show Material materials with Zugfestigkeit of 425.0 MPa | T87 | AA Standards, ASTM B209 | |||
440.0 MPa Show Material materials with Zugfestigkeit of 440.0 MPa | T87 | AA Standards, ASTM B209 | |||
475.0 MPa Show Material materials with Zugfestigkeit of 475.0 MPa | T87 | AA Standards | |||
475 MPa Show Material materials with Zugfestigkeit of 475 MPa | T87 | ||||
480.0 MPa Show Material materials with Zugfestigkeit of 480.0 MPa | T87 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T87 | ||
20 °C | 2.23e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K | T87 | AA Standards, ASTM B209 | |
100 °C | 2.23e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K | T87 | AA Standards, ASTM B209 | |
Schmelzpunkt | 540.0 °C Show Material materials with Schmelzpunkt of 540.0 °C | T87 | ||
545.0 - 645.0 °C Show Material materials with Schmelzpunkt of 545.0 - 645.0 °C | T87 | AA Standards, ASTM B209 | ||
Spezifische Wärmekapazität | 860.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 860.0 J/(kg·K) | T87 | ||
Wärmeleitfähigkeit | 113.0 - 172.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 113.0 - 172.0 W/(m·K) | T87 | AA Standards, ASTM B209 | |
120.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 120.0 W/(m·K) | T87 |
Elektrisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Elektrische Leitfähigkeit | 16000000.0 - 26000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 16000000.0 - 26000000.0 S/m | T87 | AA Standards, ASTM B209 | |
17000000 S/m Show Material materials with Elektrische Leitfähigkeit of 17000000 S/m | T87 | Typical/derived value | ||
Specific Electrical conductivity | 30.0 % IACS Show Material materials with Specific Electrical conductivity of 30.0 % IACS | T87 | Typical value | |
spezifischer Widerstand | 3.85e-08 - 6.25e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.85e-08 - 6.25e-08 Ω·m | T87 | AA Standards, ASTM B209 | |
5.7e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.7e-08 Ω·m | T87 | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 91.5 - 93.8 % Show Material materials with Aluminium of 91.5 - 93.8 % | T87 | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T87 | |
Eisen | 0.30 % Show Material materials with Eisen of 0.30 % | T87 | AA Standards, ASTM B209 |
0.3 % Show Material materials with Eisen of 0.3 % | T87 | ||
Kupfer | 5.8 - 6.8 % Show Material materials with Kupfer of 5.8 - 6.8 % | T87 | AA Standards, ASTM B209 |
Magnesium | 0.02 % Show Material materials with Magnesium of 0.02 % | T87 | AA Standards, ASTM B209 |
Mangan | 0.2 - 0.4 % Show Material materials with Mangan of 0.2 - 0.4 % | T87 | AA Standards, ASTM B209 |
Silizium | 0.2 % Show Material materials with Silizium of 0.2 % | T87 | AA Standards, ASTM B209 |
Titan | 0.02 - 0.1 % Show Material materials with Titan of 0.02 - 0.1 % | T87 | AA Standards, ASTM B209 |
Vanadium | 0.05 - 0.15 % Show Material materials with Vanadium of 0.05 - 0.15 % | T87 | AA Standards, ASTM B209 |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | T87 | AA Standards, ASTM B209 |
Zirkonium | 0.1 - 0.25 % Show Material materials with Zirkonium of 0.1 - 0.25 % | T87 | AA Standards, ASTM B209 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Betriebsschäden in Gebieten mit Zugspannungen quer zur Kornstruktur, Eingeschränkte Schäden an Laborproben (T31, T351, T3510, T3511, T37), kein Schadensfall im Betrieb, eingeschränkte Schäden bei den Labortests (T81, T851, T8510, T8511), general: sufficient, in principle it should be protected | |
General machinability | General: good to acceptable | |
Workability | general (condition): poor(T31, T351, T3510, T3511), not suitable (T37, T81, T851, T8510, T8511, T87) |