Allgemein
Property | Value | Condition |
---|---|---|
Dichte | 3.1 g/cm³ Show Material materials with Dichte of 3.1 g/cm³ | O |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Dehnung | 1.0 % Show Material materials with Dehnung of 1.0 % | O | |||
1 % Show Material materials with Dehnung of 1 % | O | Sand cast, elongation in 50 mm | |||
Elastizitätsmodul | 71.0 GPa Show Material materials with Elastizitätsmodul of 71.0 GPa | O | |||
71 GPa Show Material materials with Elastizitätsmodul of 71 GPa | O | ||||
Härte, Brinell | 70.0 [-] Show Material materials with Härte, Brinell of 70.0 [-] | O | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | O | |||
Schubmodule | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | O | |||
Streckgrenze | 120.0 MPa Show Material materials with Streckgrenze of 120.0 MPa | O | |||
124 MPa Show Material materials with Streckgrenze of 124 MPa | O | Sand cast, RP02 | |||
Zugfestigkeit | 160.0 MPa Show Material materials with Zugfestigkeit of 160.0 MPa | O | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | O | ||||
186 MPa Show Material materials with Zugfestigkeit of 186 MPa | O | Sand cast |
Thermisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | O | ||
Schmelzpunkt | 532.0 - 635.0 °C Show Material materials with Schmelzpunkt of 532.0 - 635.0 °C | O | Pink Sheets, ASTM B26, ASTM B618 | Casting |
540.0 °C Show Material materials with Schmelzpunkt of 540.0 °C | O | |||
Spezifische Wärmekapazität | 960.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 960.0 J/(kg·K) | O | ||
Wärmeleitfähigkeit | 170.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 W/(m·K) | O |
Elektrisch
Property | Value | Condition | Comment |
---|---|---|---|
Elektrische Leitfähigkeit | 25520000 S/m Show Material materials with Elektrische Leitfähigkeit of 25520000 S/m | O | Typical/Derived values |
Specific Electrical conductivity | 44 % IACS Show Material materials with Specific Electrical conductivity of 44 % IACS | O | Typical values |
spezifischer Widerstand | 4.347826086956522e-08 - 6.25e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.347826086956522e-08 - 6.25e-08 Ω·m | Typical for Cast 2xx.x Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 88.4 - 93.6 % Show Material materials with Aluminium of 88.4 - 93.6 % | O | ||
Andere | 0.15 % Show Material materials with Andere of 0.15 % | O | ||
Chrom | 0.25 % Show Material materials with Chrom of 0.25 % | O | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Eisen | 1.0 % Show Material materials with Eisen of 1.0 % | O | ||
1.00 % Show Material materials with Eisen of 1.00 % | O | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
Kupfer | 3.5 - 4.5 % Show Material materials with Kupfer of 3.5 - 4.5 % | O | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Magnesium | 1.2 - 1.8 % Show Material materials with Magnesium of 1.2 - 1.8 % | O | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Mangan | 0.35 % Show Material materials with Mangan of 0.35 % | O | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Nickel | 1.7 - 2.3 % Show Material materials with Nickel of 1.7 - 2.3 % | O | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Silizium | 0.7 % Show Material materials with Silizium of 0.7 % | O | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Titan | 0.25 % Show Material materials with Titan of 0.25 % | O | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Zink | 0.35 % Show Material materials with Zink of 0.35 % | O | Pink Sheets, ASTM B26, ASTM B618 | Casting |