Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547 |
2.8 g/cm³ Show Material materials with Dichte of 2.8 g/cm³ | H112 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Dehnung | 8.0 % Show Material materials with Dehnung of 8.0 % | H112 | AA Standards, ASTM B209, ASTM B547 | A50 |
10.0 % Show Material materials with Dehnung of 10.0 % | H112 | AA Standards, ASTM B209 | A100 | |
16.0 % Show Material materials with Dehnung of 16.0 % | H112 | AA Standards, ASTM B209, ASTM B247 | A100 | |
18.0 % Show Material materials with Dehnung of 18.0 % | H112 | AA Standards, ASTM B247 | A50 | |
20.0 % Show Material materials with Dehnung of 20.0 % | H112 | |||
22.0 % Show Material materials with Dehnung of 22.0 % | H112 | AA Standards, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | A100 | |
25.0 % Show Material materials with Dehnung of 25.0 % | H112 | AA Standards, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | A50 | |
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||
Schubmodule | 25.0 - 26.0 GPa Show Material materials with Schubmodule of 25.0 - 26.0 GPa | Typical for Wrought 3000 Series Aluminium | ||
Streckgrenze | 30.0 MPa Show Material materials with Streckgrenze of 30.0 MPa | H112 | AA Standards, ASTM B221 | RP02 |
35.0 MPa Show Material materials with Streckgrenze of 35.0 MPa | H112 | AA Standards, ASTM B211, ASTM B241, ASTM B247, ASTM B345, ASTM B483 | RP02 | |
40.0 MPa Show Material materials with Streckgrenze of 40.0 MPa | H112 | AA Standards, ASTM B209 | RP02 | |
46.0 MPa Show Material materials with Streckgrenze of 46.0 MPa | H112 | |||
70.0 MPa Show Material materials with Streckgrenze of 70.0 MPa | H112 | AA Standards, ASTM B209, ASTM B547 | RP02 | |
Zugfestigkeit | 90.0 MPa Show Material materials with Zugfestigkeit of 90.0 MPa | H112 | AA Standards, ASTM B221 | |
95.0 MPa Show Material materials with Zugfestigkeit of 95.0 MPa | H112 | AA Standards, ASTM B211, ASTM B241, ASTM B247, ASTM B345, ASTM B483 | ||
100.0 MPa Show Material materials with Zugfestigkeit of 100.0 MPa | H112 | AA Standards, ASTM B209 | ||
105.0 MPa Show Material materials with Zugfestigkeit of 105.0 MPa | H112 | AA Standards, ASTM B209 | ||
110.0 MPa Show Material materials with Zugfestigkeit of 110.0 MPa | H112 | |||
115.0 MPa Show Material materials with Zugfestigkeit of 115.0 MPa | H112 | AA Standards, ASTM B209, ASTM B547 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | H112 | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547 | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547 | |
Schmelzpunkt | 640.0 - 655.0 °C Show Material materials with Schmelzpunkt of 640.0 - 655.0 °C | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547 | |
640.0 °C Show Material materials with Schmelzpunkt of 640.0 °C | H112 | |||
Spezifische Wärmekapazität | 890.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 890.0 J/(kg·K) | H112 | ||
Wärmeleitfähigkeit | 159.0 - 193.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 159.0 - 193.0 W/(m·K) | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547 | |
180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 180.0 W/(m·K) | H112 |
Elektrisch
Property | Value | Condition | Related Standards |
---|---|---|---|
Elektrische Leitfähigkeit | 24000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000.0 - 29000000.0 S/m | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547 |
spezifischer Widerstand | 3.45e-08 - 4.17e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.45e-08 - 4.17e-08 Ω·m | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 96.8 - 99.0 % Show Material materials with Aluminium of 96.8 - 99.0 % | H112 | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | H112 | |
Eisen | 0.70 % Show Material materials with Eisen of 0.70 % | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547 |
0.7 % Show Material materials with Eisen of 0.7 % | H112 | ||
Kupfer | 0.05 - 0.2 % Show Material materials with Kupfer of 0.05 - 0.2 % | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547 |
Mangan | 1.0 - 1.5 % Show Material materials with Mangan of 1.0 - 1.5 % | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547 |
Silizium | 0.6 % Show Material materials with Silizium of 0.6 % | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547 |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | H112 | AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12), poor (H14, H16, H25) | |
Workability | general (condition): good (O, H12), acceptable (H14, H25), poor(H16, H18) |