Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | H12 | ||
2.8 g/cm³ Show Material materials with Dichte of 2.8 g/cm³ | H12 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 55.0 MPa Show Material materials with Bending Fatigue Strength of 55.0 MPa | H12 | AA Standards | |
Dauerfestigkeit | 55 MPa Show Material materials with Dauerfestigkeit of 55 MPa | H12 | for 5x10⁸ cycles | |
Dehnung | 3.0 % Show Material materials with Dehnung of 3.0 % | H12 | AA Standards, ASTM B209 | A50 |
4.0 % Show Material materials with Dehnung of 4.0 % | H12 | AA Standards, ASTM B209, ASTM B313 | A50 | |
6.0 % Show Material materials with Dehnung of 6.0 % | H12 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | A50 | |
8.0 % Show Material materials with Dehnung of 8.0 % | H12 | AA Standards, ASTM B209 | A100 | |
9.0 % Show Material materials with Dehnung of 9.0 % | H12 | AA Standards, ASTM B209, ASTM B547 | A50 | |
10.0 % Show Material materials with Dehnung of 10.0 % | H12 | AA Standards | A50 | |
11.0 % Show Material materials with Dehnung of 11.0 % | H12 | |||
15 % Show Material materials with Dehnung of 15 % | H12 | |||
18.0 % Show Material materials with Dehnung of 18.0 % | H12 | AA Standards | A100 | |
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
69 GPa Show Material materials with Elastizitätsmodul of 69 GPa | H12 | |||
Härte, Brinell | 35.0 [-] Show Material materials with Härte, Brinell of 35.0 [-] | H12 | AA Standards | |
35.0 [-] Show Material materials with Härte, Brinell of 35.0 [-] | H12 | 500 kg load, 10 mm ball | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||
Scherfestigkeit | 83.0 MPa Show Material materials with Scherfestigkeit of 83.0 MPa | H12 | ||
Schubmodule | 25.0 GPa Show Material materials with Schubmodule of 25.0 GPa | H12 | ||
Streckgrenze | 85.0 MPa Show Material materials with Streckgrenze of 85.0 MPa | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | RP02 |
110.0 MPa Show Material materials with Streckgrenze of 110.0 MPa | H12 | |||
125.0 MPa Show Material materials with Streckgrenze of 125.0 MPa | H12 | AA Standards | RP02 | |
125 MPa Show Material materials with Streckgrenze of 125 MPa | H12 | RP02 | ||
Zugfestigkeit | 115.0 MPa Show Material materials with Zugfestigkeit of 115.0 MPa | H12 | AA Standards, ASTM B211 | |
120.0 - 160.0 MPa Show Material materials with Zugfestigkeit of 120.0 - 160.0 MPa | H12 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | ||
120.0 MPa Show Material materials with Zugfestigkeit of 120.0 MPa | H12 | AA Standards, ASTM B210, ASTM B483 | ||
130.0 MPa Show Material materials with Zugfestigkeit of 130.0 MPa | H12 | AA Standards | ||
130 MPa Show Material materials with Zugfestigkeit of 130 MPa | H12 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | H12 | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
Schmelzpunkt | 640.0 - 655.0 °C Show Material materials with Schmelzpunkt of 640.0 - 655.0 °C | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
640.0 °C Show Material materials with Schmelzpunkt of 640.0 °C | H12 | |||
Spezifische Wärmekapazität | 890.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 890.0 J/(kg·K) | H12 | ||
Wärmeleitfähigkeit | 159.0 - 193.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 159.0 - 193.0 W/(m·K) | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 180.0 W/(m·K) | H12 |
Elektrisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Elektrische Leitfähigkeit | 24000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000.0 - 29000000.0 S/m | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
24000000 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000 S/m | H12 | Typical value | ||
Specific Electrical conductivity | 41.0 % IACS Show Material materials with Specific Electrical conductivity of 41.0 % IACS | H12 | Typical/Derived value | |
spezifischer Widerstand | 3.45e-08 - 4.17e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.45e-08 - 4.17e-08 Ω·m | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
4.2e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.2e-08 Ω·m | H12 | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 96.8 - 99.0 % Show Material materials with Aluminium of 96.8 - 99.0 % | H12 | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | H12 | |
Eisen | 0.70 % Show Material materials with Eisen of 0.70 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
0.7 % Show Material materials with Eisen of 0.7 % | H12 | ||
Kupfer | 0.05 - 0.2 % Show Material materials with Kupfer of 0.05 - 0.2 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Mangan | 1.0 - 1.5 % Show Material materials with Mangan of 1.0 - 1.5 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Silizium | 0.6 % Show Material materials with Silizium of 0.6 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12), poor (H14, H16, H25) | |
Workability | general (condition): good (O, H12), acceptable (H14, H25), poor(H16, H18) |