Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.72 g/cm³ Show Material materials with Dichte of 2.72 g/cm³ | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
2.72 g/cm³ Show Material materials with Dichte of 2.72 g/cm³ | H32 | ||
2.8 g/cm³ Show Material materials with Dichte of 2.8 g/cm³ | H32 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 105.0 MPa Show Material materials with Bending Fatigue Strength of 105.0 MPa | H32 | AA Standards | |
Dauerfestigkeit | 15 MPa Show Material materials with Dauerfestigkeit of 15 MPa | H32 | for 5x10⁸ cycles | |
Dehnung | 1.0 % Show Material materials with Dehnung of 1.0 % | H32 | AA Standards, ASTM B209 | A50 |
3.0 % Show Material materials with Dehnung of 3.0 % | H32 | AA Standards, ASTM B209, ASTM B313 | A50 | |
5.0 % Show Material materials with Dehnung of 5.0 % | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | A50 | |
5.0 % Show Material materials with Dehnung of 5.0 % | H32 | AA Standards, ASTM B209 | A100 | |
6.0 % Show Material materials with Dehnung of 6.0 % | H32 | AA Standards, ASTM B209, ASTM B547 | A50 | |
9.1 % Show Material materials with Dehnung of 9.1 % | H32 | |||
10.0 % Show Material materials with Dehnung of 10.0 % | H32 | AA Standards | A50 | |
13.5 % Show Material materials with Dehnung of 13.5 % | H32 | |||
15.0 % Show Material materials with Dehnung of 15.0 % | H32 | AA Standards | A100 | |
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
69 GPa Show Material materials with Elastizitätsmodul of 69 GPa | H32 | |||
Härte, Brinell | 52.0 [-] Show Material materials with Härte, Brinell of 52.0 [-] | H32 | AA Standards | |
52.0 [-] Show Material materials with Härte, Brinell of 52.0 [-] | H32 | 500 kg load, 10 mm ball | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||
Scherfestigkeit | 115.0 MPa Show Material materials with Scherfestigkeit of 115.0 MPa | H32 | ||
Schubmodule | 25.0 GPa Show Material materials with Schubmodule of 25.0 GPa | H32 | ||
Streckgrenze | 145.0 MPa Show Material materials with Streckgrenze of 145.0 MPa | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | RP02 |
170.0 MPa Show Material materials with Streckgrenze of 170.0 MPa | H32 | AA Standards | RP02 | |
170 MPa Show Material materials with Streckgrenze of 170 MPa | H32 | RP02 | ||
170.0 MPa Show Material materials with Streckgrenze of 170.0 MPa | H32 | |||
Zugfestigkeit | 190.0 - 240.0 MPa Show Material materials with Zugfestigkeit of 190.0 - 240.0 MPa | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
210.0 MPa Show Material materials with Zugfestigkeit of 210.0 MPa | H32 | |||
215.0 MPa Show Material materials with Zugfestigkeit of 215.0 MPa | H32 | AA Standards | ||
215 MPa Show Material materials with Zugfestigkeit of 215 MPa | H32 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | H32 | ||
20 °C | 2.3899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
Schmelzpunkt | 630.0 - 655.0 °C Show Material materials with Schmelzpunkt of 630.0 - 655.0 °C | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
630.0 °C Show Material materials with Schmelzpunkt of 630.0 °C | H32 | |||
Spezifische Wärmekapazität | 890.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 890.0 J/(kg·K) | H32 | ||
Wärmeleitfähigkeit | 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 W/(m·K) | H32 | ||
163 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 163 W/(m·K) | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Elektrisch
Property | Value | Condition | Related Standards |
---|---|---|---|
Elektrische Leitfähigkeit | 24000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000.0 S/m | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
spezifischer Widerstand | 4.17e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.17e-08 Ω·m | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 95.6 - 98.2 % Show Material materials with Aluminium of 95.6 - 98.2 % | H32 | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | H32 | |
Eisen | 0.70 % Show Material materials with Eisen of 0.70 % | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
0.7 % Show Material materials with Eisen of 0.7 % | H32 | ||
Kupfer | 0.25 % Show Material materials with Kupfer of 0.25 % | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Magnesium | 0.8 - 1.3 % Show Material materials with Magnesium of 0.8 - 1.3 % | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Mangan | 1.0 - 1.5 % Show Material materials with Mangan of 1.0 - 1.5 % | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Silizium | 0.3 % Show Material materials with Silizium of 0.3 % | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 |
Technological properties
Property | ||
---|---|---|
Brazing | general: Lötbar mit speziellen Techniken oder bei bestimmten Anwendungen | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O, H32), sufficient (H34, H36, H38) | |
Workability | general (condition): good (O), acceptable (H32, H34), poor(H36, H38) |