Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | O | AA Standards |
2.8 g/cm³ Show Material materials with Dichte of 2.8 g/cm³ | O |
Mechanisch
Property | Value | Condition | Comment |
---|---|---|---|
Dehnung | 26.0 % Show Material materials with Dehnung of 26.0 % | O | |
Elastizitätsmodul | 72.0 GPa Show Material materials with Elastizitätsmodul of 72.0 GPa | O | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | |
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | |
Schubmodule | 25.0 - 26.0 GPa Show Material materials with Schubmodule of 25.0 - 26.0 GPa | Typical for Wrought 3000 Series Aluminium | |
Streckgrenze | 40.0 MPa Show Material materials with Streckgrenze of 40.0 MPa | O | |
Zugfestigkeit | 110.0 MPa Show Material materials with Zugfestigkeit of 110.0 MPa | O |
Thermisch
Property | Value | Condition |
---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | O |
Schmelzpunkt | 640.0 °C Show Material materials with Schmelzpunkt of 640.0 °C | O |
Spezifische Wärmekapazität | 890.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 890.0 J/(kg·K) | O |
Wärmeleitfähigkeit | 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 W/(m·K) | O |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 23000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 29000000.0 S/m | Typical for Wrought 3000 Series Aluminium |
spezifischer Widerstand | 3.4e-08 - 4.2e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 4.2e-08 Ω·m | Typical for Wrought 3000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 96.3 - 99.1 % Show Material materials with Aluminium of 96.3 - 99.1 % | O | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | O | |
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | O | AA Standards |
Eisen | 0.70 % Show Material materials with Eisen of 0.70 % | O | AA Standards |
0.7 % Show Material materials with Eisen of 0.7 % | O | ||
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | O | AA Standards |
Magnesium | 0.3 % Show Material materials with Magnesium of 0.3 % | O | AA Standards |
Mangan | 0.9 - 1.5 % Show Material materials with Mangan of 0.9 - 1.5 % | O | AA Standards |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | O | AA Standards |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | O | |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | O | AA Standards |
Zirkonium | 0.1 % Show Material materials with Zirkonium of 0.1 % | O |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |