Allgemein
Property | Value | Condition |
---|---|---|
Dichte | 3.0 g/cm³ Show Material materials with Dichte of 3.0 g/cm³ | T5 |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Compressive yield strength | 138 MPa Show Material materials with Compressive yield strength of 138 MPa | T5 | |||
Dauerfestigkeit | 76 MPa Show Material materials with Dauerfestigkeit of 76 MPa | T5 | for 5x10⁸ cycles, R.R. Moore type test | ||
Dehnung | 1.5 % Show Material materials with Dehnung of 1.5 % | T5 | Sand cast, elongation in 50 mm | ||
1.8 % Show Material materials with Dehnung of 1.8 % | T5 | ||||
Elastizitätsmodul | 74 GPa Show Material materials with Elastizitätsmodul of 74 GPa | T5 | |||
78.0 GPa Show Material materials with Elastizitätsmodul of 78.0 GPa | T5 | ||||
Härte, Brinell | 80 [-] Show Material materials with Härte, Brinell of 80 [-] | T5 | 500 kg load, 10 mm b | ||
80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | T5 | Pink Sheets, ASTM B26 | Casting | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | T5 | |||
Scherfestigkeit | 165 MPa Show Material materials with Scherfestigkeit of 165 MPa | T5 | |||
Schubmodule | 28.0 GPa Show Material materials with Schubmodule of 28.0 GPa | T5 | |||
Streckgrenze | 179 MPa Show Material materials with Streckgrenze of 179 MPa | T5 | Sand cast, RP02 | ||
180.0 MPa Show Material materials with Streckgrenze of 180.0 MPa | T5 | ||||
Zugfestigkeit | 170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | T5 | Pink Sheets, ASTM B26 | Casting | |
200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | T5 | ||||
207 MPa Show Material materials with Zugfestigkeit of 207 MPa | T5 | Sand cast |
Thermisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T5 | ||
Schmelzpunkt | 510.0 - 607.0 °C Show Material materials with Schmelzpunkt of 510.0 - 607.0 °C | T5 | Pink Sheets, ASTM B26 | Casting |
540.0 °C Show Material materials with Schmelzpunkt of 540.0 °C | T5 | |||
Spezifische Wärmekapazität | 860.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 860.0 J/(kg·K) | T5 | ||
Wärmeleitfähigkeit | 110.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 110.0 W/(m·K) | T5 |
Elektrisch
Property | Value | Condition | Comment |
---|---|---|---|
spezifischer Widerstand | 6.39e-08 Ω·m Show Material materials with spezifischer Widerstand of 6.39e-08 Ω·m | T5 | Typical values |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 85.8 - 91.5 % Show Material materials with Aluminium of 85.8 - 91.5 % | T5 | ||
Andere | 0.5 % Show Material materials with Andere of 0.5 % | T5 | ||
Eisen | 1.0 % Show Material materials with Eisen of 1.0 % | T5 | ||
1.00 % Show Material materials with Eisen of 1.00 % | T5 | Pink Sheets, ASTM B26 | Casting | |
Kupfer | 3.0 - 4.0 % Show Material materials with Kupfer of 3.0 - 4.0 % | T5 | Pink Sheets, ASTM B26 | Casting |
Magnesium | 0.1 % Show Material materials with Magnesium of 0.1 % | T5 | Pink Sheets, ASTM B26 | Casting |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | T5 | Pink Sheets, ASTM B26 | Casting |
Nickel | 0.35 % Show Material materials with Nickel of 0.35 % | T5 | Pink Sheets, ASTM B26 | Casting |
Silizium | 5.5 - 6.5 % Show Material materials with Silizium of 5.5 - 6.5 % | T5 | Pink Sheets, ASTM B26 | Casting |
Titan | 0.25 % Show Material materials with Titan of 0.25 % | T5 | Pink Sheets, ASTM B26 | Casting |
Zink | 1.0 % Show Material materials with Zink of 1.0 % | T5 | Pink Sheets, ASTM B26 | Casting |