Allgemein
Property | Value | Condition |
---|---|---|
Dichte | 2.8 g/cm³ Show Material materials with Dichte of 2.8 g/cm³ | T6 |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Compressive yield strength | 179.0 - 186.0 MPa Show Material materials with Compressive yield strength of 179.0 - 186.0 MPa | T6 | ||||
Dauerfestigkeit | 62.0 - 70.0 MPa Show Material materials with Dauerfestigkeit of 62.0 - 70.0 MPa | T6 | for 5x10⁸ cycles, R.R. Moore type test | |||
Dehnung | 2.0 % Show Material materials with Dehnung of 2.0 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | A100 | |
2.6 % Show Material materials with Dehnung of 2.6 % | T6 | |||||
25 °C | 3 % Show Material materials with Dehnung of 3 % | T6 | Sand cast, elongation in 50 mm | |||
150 °C | 1.5 % Show Material materials with Dehnung of 1.5 % | T6 | Sand cast, elongation in 50 mm | |||
205 °C | 8 % Show Material materials with Dehnung of 8 % | T6 | Sand cast, elongation in 50 mm | |||
260 °C | 16 % Show Material materials with Dehnung of 16 % | T6 | Sand cast, elongation in 50 mm | |||
315 °C | 36 % Show Material materials with Dehnung of 36 % | T6 | Sand cast, elongation in 50 mm | |||
Elastizitätsmodul | 76.0 GPa Show Material materials with Elastizitätsmodul of 76.0 GPa | T6 | ||||
25 °C | 70.3 GPa Show Material materials with Elastizitätsmodul of 70.3 GPa | T6 | ||||
150 °C | 67.6 GPa Show Material materials with Elastizitätsmodul of 67.6 GPa | T6 | ||||
204 °C | 64.1 GPa Show Material materials with Elastizitätsmodul of 64.1 GPa | T6 | ||||
260 °C | 56.5 GPa Show Material materials with Elastizitätsmodul of 56.5 GPa | T6 | ||||
Härte, Brinell | 80.0 - 90.0 [-] Show Material materials with Härte, Brinell of 80.0 - 90.0 [-] | T6 | 500 kg load, 10 mm b | |||
80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | T6 | ||||
Scherfestigkeit | 193.0 - 234.0 MPa Show Material materials with Scherfestigkeit of 193.0 - 234.0 MPa | T6 | ||||
Schubmodule | 26.2 GPa Show Material materials with Schubmodule of 26.2 GPa | T6 | ||||
Streckgrenze | 140.0 MPa Show Material materials with Streckgrenze of 140.0 MPa | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | RP02 | |
170.0 MPa Show Material materials with Streckgrenze of 170.0 MPa | T6 | |||||
25 °C | 170 MPa Show Material materials with Streckgrenze of 170 MPa | T6 | Sand cast, RP02 | |||
150 °C | 170 MPa Show Material materials with Streckgrenze of 170 MPa | T6 | Sand cast, RP02 | |||
205 °C | 90 MPa Show Material materials with Streckgrenze of 90 MPa | T6 | Sand cast, RP02 | |||
260 °C | 35 MPa Show Material materials with Streckgrenze of 35 MPa | T6 | Sand cast, RP02 | |||
315 °C | 20 MPa Show Material materials with Streckgrenze of 20 MPa | T6 | Sand cast, RP02 | |||
Zugfestigkeit | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | ||
260.0 MPa Show Material materials with Zugfestigkeit of 260.0 MPa | T6 | |||||
25 °C | 240 MPa Show Material materials with Zugfestigkeit of 240 MPa | T6 | Sand cast | |||
150 °C | 230 MPa Show Material materials with Zugfestigkeit of 230 MPa | T6 | Sand cast | |||
205 °C | 115 MPa Show Material materials with Zugfestigkeit of 115 MPa | T6 | Sand cast | |||
260 °C | 65 MPa Show Material materials with Zugfestigkeit of 65 MPa | T6 | Sand cast | |||
315 °C | 40 MPa Show Material materials with Zugfestigkeit of 40 MPa | T6 | Sand cast |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T6 | ||||
100 °C | 0.0000223 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.0000223 1/K | T6 | nominal value between 20°C and the mentioned temperature | |||
300 °C | 0.0000247 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.0000247 1/K | T6 | nominal value between 20°C and the mentioned temperature | |||
Schmelzpunkt | 546.0 - 621.0 °C Show Material materials with Schmelzpunkt of 546.0 - 621.0 °C | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | ||
560.0 °C Show Material materials with Schmelzpunkt of 560.0 °C | T6 | |||||
Spezifische Wärmekapazität | 880.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 880.0 J/(kg·K) | T6 | ||||
100 °C | 960 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 960 J/(kg·K) | T6 | derived value | |||
Wärmeleitfähigkeit | 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 150.0 W/(m·K) | T6 | ||||
25 °C | 142 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 142 W/(m·K) | T6 | nominal value |
Elektrisch
Property | Value | Condition | Comment |
---|---|---|---|
Elektrische Leitfähigkeit | 22619999.999999996 S/m Show Material materials with Elektrische Leitfähigkeit of 22619999.999999996 S/m | T6 | Typical/Derived values |
Specific Electrical conductivity | 39 % IACS Show Material materials with Specific Electrical conductivity of 39 % IACS | T6 | Typical values |
spezifischer Widerstand | 4.42e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.42e-08 Ω·m | T6 | Typical values |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 90.3 - 94.1 % Show Material materials with Aluminium of 90.3 - 94.1 % | T6 | ||
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T6 | ||
Chrom | 0.25 % Show Material materials with Chrom of 0.25 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Eisen | 0.6 % Show Material materials with Eisen of 0.6 % | T6 | ||
0.60 % Show Material materials with Eisen of 0.60 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
Kupfer | 1.0 - 1.5 % Show Material materials with Kupfer of 1.0 - 1.5 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Magnesium | 0.4 - 0.6 % Show Material materials with Magnesium of 0.4 - 0.6 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Silizium | 4.5 - 5.5 % Show Material materials with Silizium of 4.5 - 5.5 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Titan | 0.25 % Show Material materials with Titan of 0.25 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Zink | 0.35 % Show Material materials with Zink of 0.35 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |