Allgemein
Property | Value | Condition |
---|---|---|
Dichte | 2.8 g/cm³ Show Material materials with Dichte of 2.8 g/cm³ | T71 |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Compressive yield strength | 248 MPa Show Material materials with Compressive yield strength of 248 MPa | T71 | ||||
Dauerfestigkeit | 70 MPa Show Material materials with Dauerfestigkeit of 70 MPa | T71 | for 5x10⁸ cycles, R.R. Moore type test | |||
Dehnung | -195 °C | 1.5 % Show Material materials with Dehnung of 1.5 % | T71 | Sand cast, elongation in 50 mm | ||
-80 °C | 1.5 % Show Material materials with Dehnung of 1.5 % | T71 | Sand cast, elongation in 50 mm | |||
-28 °C | 1.5 % Show Material materials with Dehnung of 1.5 % | T71 | Sand cast, elongation in 50 mm | |||
1.5 % Show Material materials with Dehnung of 1.5 % | T71 | |||||
24 °C | 1.5 % Show Material materials with Dehnung of 1.5 % | T71 | Sand cast, elongation in 50 mm | |||
100 °C | 2 % Show Material materials with Dehnung of 2 % | T71 | Sand cast, elongation in 50 mm | |||
150 °C | 3 % Show Material materials with Dehnung of 3 % | T71 | Sand cast, elongation in 50 mm | |||
205 °C | 8 % Show Material materials with Dehnung of 8 % | T71 | Sand cast, elongation in 50 mm | |||
260 °C | 16 % Show Material materials with Dehnung of 16 % | T71 | Sand cast, elongation in 50 mm | |||
315 °C | 36 % Show Material materials with Dehnung of 36 % | T71 | Sand cast, elongation in 50 mm | |||
371 °C | 50 % Show Material materials with Dehnung of 50 % | T71 | Sand cast, elongation in 50 mm | |||
Elastizitätsmodul | 76.0 GPa Show Material materials with Elastizitätsmodul of 76.0 GPa | T71 | ||||
25 °C | 70.3 GPa Show Material materials with Elastizitätsmodul of 70.3 GPa | T71 | ||||
150 °C | 67.6 GPa Show Material materials with Elastizitätsmodul of 67.6 GPa | T71 | ||||
204 °C | 64.1 GPa Show Material materials with Elastizitätsmodul of 64.1 GPa | T71 | ||||
260 °C | 56.5 GPa Show Material materials with Elastizitätsmodul of 56.5 GPa | T71 | ||||
Härte, Brinell | 75 [-] Show Material materials with Härte, Brinell of 75 [-] | T71 | 500 kg load, 10 mm b | |||
75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | T71 | Pink Sheets, ASTM B618 | Casting | |||
80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | T71 | Pink Sheets, ASTM B108 | Casting | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | T71 | ||||
Scherfestigkeit | 241 MPa Show Material materials with Scherfestigkeit of 241 MPa | T71 | ||||
Schubmodule | 26.2 GPa Show Material materials with Schubmodule of 26.2 GPa | T71 | ||||
Streckgrenze | -195 °C | 235 MPa Show Material materials with Streckgrenze of 235 MPa | T71 | Sand cast, RP02 | ||
-80 °C | 220 MPa Show Material materials with Streckgrenze of 220 MPa | T71 | Sand cast, RP02 | |||
-28 °C | 215 MPa Show Material materials with Streckgrenze of 215 MPa | T71 | Sand cast, RP02 | |||
150.0 MPa Show Material materials with Streckgrenze of 150.0 MPa | T71 | Pink Sheets, ASTM B618 | Casting | RP02 | ||
185.0 MPa Show Material materials with Streckgrenze of 185.0 MPa | T71 | Pink Sheets, ASTM B108 | Casting | RP02 | ||
190.0 MPa Show Material materials with Streckgrenze of 190.0 MPa | T71 | |||||
24 °C | 200 MPa Show Material materials with Streckgrenze of 200 MPa | T71 | Sand cast, RP02 | |||
100 °C | 193 MPa Show Material materials with Streckgrenze of 193 MPa | T71 | Sand cast, RP02 | |||
150 °C | 180 MPa Show Material materials with Streckgrenze of 180 MPa | T71 | Sand cast, RP02 | |||
205 °C | 90 MPa Show Material materials with Streckgrenze of 90 MPa | T71 | Sand cast, RP02 | |||
260 °C | 35 MPa Show Material materials with Streckgrenze of 35 MPa | T71 | Sand cast, RP02 | |||
315 °C | 21 MPa Show Material materials with Streckgrenze of 21 MPa | T71 | Sand cast, RP02 | |||
371 °C | 14 MPa Show Material materials with Streckgrenze of 14 MPa | T71 | Sand cast, RP02 | |||
Zugfestigkeit | -195 °C | 282 MPa Show Material materials with Zugfestigkeit of 282 MPa | T71 | Sand cast | ||
-80 °C | 255 MPa Show Material materials with Zugfestigkeit of 255 MPa | T71 | Sand cast | |||
-28 °C | 248 MPa Show Material materials with Zugfestigkeit of 248 MPa | T71 | Sand cast | |||
200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | T71 | |||||
205.0 MPa Show Material materials with Zugfestigkeit of 205.0 MPa | T71 | Pink Sheets, ASTM B618 | Casting | |||
235.0 MPa Show Material materials with Zugfestigkeit of 235.0 MPa | T71 | Pink Sheets, ASTM B108 | Casting | |||
24 °C | 240 MPa Show Material materials with Zugfestigkeit of 240 MPa | T71 | Sand cast | |||
100 °C | 235 MPa Show Material materials with Zugfestigkeit of 235 MPa | T71 | Sand cast | |||
150 °C | 207 MPa Show Material materials with Zugfestigkeit of 207 MPa | T71 | Sand cast | |||
205 °C | 117 MPa Show Material materials with Zugfestigkeit of 117 MPa | T71 | Sand cast | |||
260 °C | 67 MPa Show Material materials with Zugfestigkeit of 67 MPa | T71 | Sand cast | |||
315 °C | 41 MPa Show Material materials with Zugfestigkeit of 41 MPa | T71 | Sand cast | |||
371 °C | 25 MPa Show Material materials with Zugfestigkeit of 25 MPa | T71 | Sand cast |
Thermisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T71 | ||
Schmelzpunkt | 546.0 - 621.0 °C Show Material materials with Schmelzpunkt of 546.0 - 621.0 °C | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
560.0 °C Show Material materials with Schmelzpunkt of 560.0 °C | T71 | |||
Spezifische Wärmekapazität | 880.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 880.0 J/(kg·K) | T71 | ||
Wärmeleitfähigkeit | 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 W/(m·K) | T71 |
Elektrisch
Property | Value | Condition | Comment |
---|---|---|---|
Elektrische Leitfähigkeit | 20880000 S/m Show Material materials with Elektrische Leitfähigkeit of 20880000 S/m | T71 | Typical/Derived values |
Specific Electrical conductivity | 36 % IACS Show Material materials with Specific Electrical conductivity of 36 % IACS | T71 | Typical values |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 90.3 - 94.1 % Show Material materials with Aluminium of 90.3 - 94.1 % | T71 | ||
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T71 | ||
Chrom | 0.25 % Show Material materials with Chrom of 0.25 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Eisen | 0.6 % Show Material materials with Eisen of 0.6 % | T71 | ||
0.60 % Show Material materials with Eisen of 0.60 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting | |
Kupfer | 1.0 - 1.5 % Show Material materials with Kupfer of 1.0 - 1.5 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Magnesium | 0.4 - 0.6 % Show Material materials with Magnesium of 0.4 - 0.6 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Silizium | 4.5 - 5.5 % Show Material materials with Silizium of 4.5 - 5.5 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Titan | 0.25 % Show Material materials with Titan of 0.25 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Zink | 0.35 % Show Material materials with Zink of 0.35 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |