Allgemein
Property | Value | Condition |
---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | T51 |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Compressive yield strength | 145 MPa Show Material materials with Compressive yield strength of 145 MPa | T51 | |||
Dauerfestigkeit | 55 MPa Show Material materials with Dauerfestigkeit of 55 MPa | T51 | for 5x10⁸ cycles, R.R. Moore type test | ||
Dehnung | 2.0 % Show Material materials with Dehnung of 2.0 % | T51 | |||
2 % Show Material materials with Dehnung of 2 % | T51 | Sand cast, elongation in 50 mm | |||
Elastizitätsmodul | 72.0 GPa Show Material materials with Elastizitätsmodul of 72.0 GPa | T51 | |||
72.4 GPa Show Material materials with Elastizitätsmodul of 72.4 GPa | T51 | ||||
Härte, Brinell | 60 [-] Show Material materials with Härte, Brinell of 60 [-] | T51 | 500 kg load, 10 mm b | ||
60.0 [-] Show Material materials with Härte, Brinell of 60.0 [-] | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | T51 | |||
Scherfestigkeit | 138 MPa Show Material materials with Scherfestigkeit of 138 MPa | T51 | |||
Schubmodule | 27.2 GPa Show Material materials with Schubmodule of 27.2 GPa | T51 | |||
Streckgrenze | 110.0 MPa Show Material materials with Streckgrenze of 110.0 MPa | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting | RP02 |
130.0 MPa Show Material materials with Streckgrenze of 130.0 MPa | T51 | ||||
138 MPa Show Material materials with Streckgrenze of 138 MPa | T51 | Sand cast, RP02 | |||
Zugfestigkeit | 160.0 MPa Show Material materials with Zugfestigkeit of 160.0 MPa | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
172 MPa Show Material materials with Zugfestigkeit of 172 MPa | T51 | Sand cast | |||
180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | T51 |
Thermisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T51 | ||
Schmelzpunkt | 557.0 - 613.0 °C Show Material materials with Schmelzpunkt of 557.0 - 613.0 °C | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
570.0 °C Show Material materials with Schmelzpunkt of 570.0 °C | T51 | |||
Spezifische Wärmekapazität | 970.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 970.0 J/(kg·K) | T51 | ||
Wärmeleitfähigkeit | 170.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 W/(m·K) | T51 |
Elektrisch
Property | Value | Condition | Comment |
---|---|---|---|
Elektrische Leitfähigkeit | 24939999.999999996 S/m Show Material materials with Elektrische Leitfähigkeit of 24939999.999999996 S/m | T51 | Typical/Derived values |
Specific Electrical conductivity | 43 % IACS Show Material materials with Specific Electrical conductivity of 43 % IACS | T51 | Typical values |
spezifischer Widerstand | 4.0099999999999995e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.0099999999999995e-08 Ω·m | T51 | Typical values |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 90.1 - 93.3 % Show Material materials with Aluminium of 90.1 - 93.3 % | T51 | ||
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T51 | ||
Eisen | 0.6 % Show Material materials with Eisen of 0.6 % | T51 | ||
0.60 % Show Material materials with Eisen of 0.60 % | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
Kupfer | 0.25 % Show Material materials with Kupfer of 0.25 % | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Magnesium | 0.2 - 0.45 % Show Material materials with Magnesium of 0.2 - 0.45 % | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Mangan | 0.35 % Show Material materials with Mangan of 0.35 % | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Silizium | 6.5 - 7.5 % Show Material materials with Silizium of 6.5 - 7.5 % | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Titan | 0.25 % Show Material materials with Titan of 0.25 % | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Zink | 0.35 % Show Material materials with Zink of 0.35 % | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting |