Allgemein
Property | Value | Condition |
---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | T7 |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Compressive yield strength | 165.0 - 214.0 MPa Show Material materials with Compressive yield strength of 165.0 - 214.0 MPa | T7 | ||||
Dauerfestigkeit | 62.0 - 76.0 MPa Show Material materials with Dauerfestigkeit of 62.0 - 76.0 MPa | T7 | for 5x10⁸ cycles, R.R. Moore type test | |||
Dehnung | -195 °C | 2 % Show Material materials with Dehnung of 2 % | T7 | Sand cast, elongation in 50 mm | ||
-80 °C | 2 % Show Material materials with Dehnung of 2 % | T7 | Sand cast, elongation in 50 mm | |||
-28 °C | 2 % Show Material materials with Dehnung of 2 % | T7 | Sand cast, elongation in 50 mm | |||
3.0 % Show Material materials with Dehnung of 3.0 % | T7 | Pink Sheets, ASTM B26 | Casting | A100 | ||
3.4 % Show Material materials with Dehnung of 3.4 % | T7 | |||||
24 °C | 2 % Show Material materials with Dehnung of 2 % | T7 | Sand cast, elongation in 50 mm | |||
100 °C | 2 % Show Material materials with Dehnung of 2 % | T7 | Sand cast, elongation in 50 mm | |||
150 °C | 6 % Show Material materials with Dehnung of 6 % | T7 | Sand cast, elongation in 50 mm | |||
205 °C | 18 % Show Material materials with Dehnung of 18 % | T7 | Sand cast, elongation in 50 mm | |||
260 °C | 35 % Show Material materials with Dehnung of 35 % | T7 | Sand cast, elongation in 50 mm | |||
315 °C | 60 % Show Material materials with Dehnung of 60 % | T7 | Sand cast, elongation in 50 mm | |||
371 °C | 80 % Show Material materials with Dehnung of 80 % | T7 | Sand cast, elongation in 50 mm | |||
Elastizitätsmodul | 72.0 GPa Show Material materials with Elastizitätsmodul of 72.0 GPa | T7 | ||||
72.4 GPa Show Material materials with Elastizitätsmodul of 72.4 GPa | T7 | |||||
Härte, Brinell | 60.0 [-] Show Material materials with Härte, Brinell of 60.0 [-] | T7 | Pink Sheets, ASTM B26 | Casting | ||
70.0 - 75.0 [-] Show Material materials with Härte, Brinell of 70.0 - 75.0 [-] | T7 | 500 kg load, 10 mm b | ||||
75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | T7 | ||||
Scherfestigkeit | 165 MPa Show Material materials with Scherfestigkeit of 165 MPa | T7 | ||||
Schubmodule | 27.2 GPa Show Material materials with Schubmodule of 27.2 GPa | T7 | ||||
Streckgrenze | -195 °C | 240 MPa Show Material materials with Streckgrenze of 240 MPa | T7 | Sand cast, RP02 | ||
-80 °C | 220 MPa Show Material materials with Streckgrenze of 220 MPa | T7 | Sand cast, RP02 | |||
-28 °C | 215 MPa Show Material materials with Streckgrenze of 215 MPa | T7 | Sand cast, RP02 | |||
125.0 MPa Show Material materials with Streckgrenze of 125.0 MPa | T7 | Pink Sheets, ASTM B26 | Casting | RP02 | ||
190.0 MPa Show Material materials with Streckgrenze of 190.0 MPa | T7 | |||||
24 °C | 207 MPa Show Material materials with Streckgrenze of 207 MPa | T7 | Sand cast, RP02 | |||
100 °C | 193 MPa Show Material materials with Streckgrenze of 193 MPa | T7 | Sand cast, RP02 | |||
150 °C | 138 MPa Show Material materials with Streckgrenze of 138 MPa | T7 | Sand cast, RP02 | |||
205 °C | 58 MPa Show Material materials with Streckgrenze of 58 MPa | T7 | Sand cast, RP02 | |||
260 °C | 34 MPa Show Material materials with Streckgrenze of 34 MPa | T7 | Sand cast, RP02 | |||
315 °C | 21 MPa Show Material materials with Streckgrenze of 21 MPa | T7 | Sand cast, RP02 | |||
371 °C | 14 MPa Show Material materials with Streckgrenze of 14 MPa | T7 | Sand cast, RP02 | |||
Zugfestigkeit | -195 °C | 283 MPa Show Material materials with Zugfestigkeit of 283 MPa | T7 | Sand cast | ||
-80 °C | 248 MPa Show Material materials with Zugfestigkeit of 248 MPa | T7 | Sand cast | |||
-28 °C | 235 MPa Show Material materials with Zugfestigkeit of 235 MPa | T7 | Sand cast | |||
170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | T7 | Pink Sheets, ASTM B26 | Casting | |||
215.0 MPa Show Material materials with Zugfestigkeit of 215.0 MPa | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |||
230.0 MPa Show Material materials with Zugfestigkeit of 230.0 MPa | T7 | |||||
24 °C | 235 MPa Show Material materials with Zugfestigkeit of 235 MPa | T7 | Sand cast | |||
100 °C | 207 MPa Show Material materials with Zugfestigkeit of 207 MPa | T7 | Sand cast | |||
150 °C | 160 MPa Show Material materials with Zugfestigkeit of 160 MPa | T7 | Sand cast | |||
205 °C | 83 MPa Show Material materials with Zugfestigkeit of 83 MPa | T7 | Sand cast | |||
260 °C | 53 MPa Show Material materials with Zugfestigkeit of 53 MPa | T7 | Sand cast | |||
315 °C | 28 MPa Show Material materials with Zugfestigkeit of 28 MPa | T7 | Sand cast | |||
371 °C | 17 MPa Show Material materials with Zugfestigkeit of 17 MPa | T7 | Sand cast |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T7 | ||||
Schmelzpunkt | 557.0 - 613.0 °C Show Material materials with Schmelzpunkt of 557.0 - 613.0 °C | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting | ||
570.0 °C Show Material materials with Schmelzpunkt of 570.0 °C | T7 | |||||
Spezifische Wärmekapazität | 970.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 970.0 J/(kg·K) | T7 | ||||
Wärmeleitfähigkeit | 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 150.0 W/(m·K) | T7 | ||||
25 °C | 155 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 155 W/(m·K) | T7 | nominal value |
Elektrisch
Property | Value | Condition | Comment |
---|---|---|---|
Elektrische Leitfähigkeit | 24000000 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000 S/m | T7 | Typical/Derived values |
Specific Electrical conductivity | 40.0 - 43.0 % IACS Show Material materials with Specific Electrical conductivity of 40.0 - 43.0 % IACS | T7 | Typical values |
spezifischer Widerstand | 4.3099999999999996e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.3099999999999996e-08 Ω·m | T7 | Typical values |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 90.1 - 93.3 % Show Material materials with Aluminium of 90.1 - 93.3 % | T7 | ||
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T7 | ||
Eisen | 0.6 % Show Material materials with Eisen of 0.6 % | T7 | ||
0.60 % Show Material materials with Eisen of 0.60 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
Kupfer | 0.25 % Show Material materials with Kupfer of 0.25 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Magnesium | 0.2 - 0.45 % Show Material materials with Magnesium of 0.2 - 0.45 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Mangan | 0.35 % Show Material materials with Mangan of 0.35 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Silizium | 6.5 - 7.5 % Show Material materials with Silizium of 6.5 - 7.5 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Titan | 0.25 % Show Material materials with Titan of 0.25 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Zink | 0.35 % Show Material materials with Zink of 0.35 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |