Allgemein
Property | Value | Condition |
---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | T71 |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Dauerfestigkeit | 59 MPa Show Material materials with Dauerfestigkeit of 59 MPa | T71 | for 5x10⁸ cycles, R.R. Moore type test | ||
Dehnung | 3.0 % Show Material materials with Dehnung of 3.0 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting | A100 |
3.5 % Show Material materials with Dehnung of 3.5 % | T71 | ||||
3.5 % Show Material materials with Dehnung of 3.5 % | T71 | Sand cast, elongation in 50 mm | |||
Elastizitätsmodul | 72.0 GPa Show Material materials with Elastizitätsmodul of 72.0 GPa | T71 | |||
72.4 GPa Show Material materials with Elastizitätsmodul of 72.4 GPa | T71 | ||||
Härte, Brinell | 60 [-] Show Material materials with Härte, Brinell of 60 [-] | T71 | 500 kg load, 10 mm b | ||
60.0 [-] Show Material materials with Härte, Brinell of 60.0 [-] | T71 | Pink Sheets, ASTM B618 | Casting | ||
70.0 [-] Show Material materials with Härte, Brinell of 70.0 [-] | T71 | Pink Sheets, ASTM B108 | Casting | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | T71 | |||
Scherfestigkeit | 138 MPa Show Material materials with Scherfestigkeit of 138 MPa | T71 | |||
Schubmodule | 27.2 GPa Show Material materials with Schubmodule of 27.2 GPa | T71 | |||
Streckgrenze | 125.0 MPa Show Material materials with Streckgrenze of 125.0 MPa | T71 | Pink Sheets, ASTM B618 | Casting | RP02 |
140.0 MPa Show Material materials with Streckgrenze of 140.0 MPa | T71 | ||||
145 MPa Show Material materials with Streckgrenze of 145 MPa | T71 | Sand cast, RP02 | |||
Zugfestigkeit | 150.0 MPa Show Material materials with Zugfestigkeit of 150.0 MPa | T71 | |||
170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting | ||
193 MPa Show Material materials with Zugfestigkeit of 193 MPa | T71 | Sand cast |
Thermisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T71 | ||
Schmelzpunkt | 557.0 - 613.0 °C Show Material materials with Schmelzpunkt of 557.0 - 613.0 °C | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
570.0 °C Show Material materials with Schmelzpunkt of 570.0 °C | T71 | |||
Spezifische Wärmekapazität | 970.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 970.0 J/(kg·K) | T71 | ||
Wärmeleitfähigkeit | 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 W/(m·K) | T71 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 90.1 - 93.3 % Show Material materials with Aluminium of 90.1 - 93.3 % | T71 | ||
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T71 | ||
Eisen | 0.6 % Show Material materials with Eisen of 0.6 % | T71 | ||
0.60 % Show Material materials with Eisen of 0.60 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting | |
Kupfer | 0.25 % Show Material materials with Kupfer of 0.25 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Magnesium | 0.2 - 0.45 % Show Material materials with Magnesium of 0.2 - 0.45 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Mangan | 0.35 % Show Material materials with Mangan of 0.35 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Silizium | 6.5 - 7.5 % Show Material materials with Silizium of 6.5 - 7.5 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Titan | 0.25 % Show Material materials with Titan of 0.25 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |
Zink | 0.35 % Show Material materials with Zink of 0.35 % | T71 | Pink Sheets, ASTM B108, ASTM B618 | Casting |