Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H36 | ||
2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H36 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 95.0 MPa Show Material materials with Bending Fatigue Strength of 95.0 MPa | H36 | AA Standards | |
Dauerfestigkeit | 97 MPa Show Material materials with Dauerfestigkeit of 97 MPa | H36 | for 5x10⁸ cycles | |
Dehnung | 2.0 % Show Material materials with Dehnung of 2.0 % | H36 | AA Standards, ASTM B209 | A50 |
3.0 % Show Material materials with Dehnung of 3.0 % | H36 | AA Standards, ASTM B209, ASTM B313 | A50 | |
4.0 % Show Material materials with Dehnung of 4.0 % | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | A50 | |
4.7 % Show Material materials with Dehnung of 4.7 % | H36 | |||
7.0 % Show Material materials with Dehnung of 7.0 % | H36 | AA Standards | A50 | |
7 % Show Material materials with Dehnung of 7 % | H36 | |||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | |
69 GPa Show Material materials with Elastizitätsmodul of 69 GPa | H36 | |||
Härte, Brinell | 58.0 [-] Show Material materials with Härte, Brinell of 58.0 [-] | H36 | AA Standards | |
58.0 [-] Show Material materials with Härte, Brinell of 58.0 [-] | H36 | 500 kg load, 10 mm ball | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||
Scherfestigkeit | 130.0 MPa Show Material materials with Scherfestigkeit of 130.0 MPa | H36 | ||
Schubmodule | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | H36 | ||
Streckgrenze | 150.0 MPa Show Material materials with Streckgrenze of 150.0 MPa | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | RP02 |
180.0 MPa Show Material materials with Streckgrenze of 180.0 MPa | H36 | AA Standards | RP02 | |
180 MPa Show Material materials with Streckgrenze of 180 MPa | H36 | RP02 | ||
180.0 MPa Show Material materials with Streckgrenze of 180.0 MPa | H36 | |||
Zugfestigkeit | 185.0 - 230.0 MPa Show Material materials with Zugfestigkeit of 185.0 - 230.0 MPa | H36 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
185.0 MPa Show Material materials with Zugfestigkeit of 185.0 MPa | H36 | AA Standards, ASTM B210, ASTM B483 | ||
205.0 MPa Show Material materials with Zugfestigkeit of 205.0 MPa | H36 | AA Standards | ||
205 MPa Show Material materials with Zugfestigkeit of 205 MPa | H36 | |||
210.0 MPa Show Material materials with Zugfestigkeit of 210.0 MPa | H36 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | H36 | |||
20 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | ||
100 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||
Schmelzpunkt | 625.0 - 650.0 °C Show Material materials with Schmelzpunkt of 625.0 - 650.0 °C | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | ||
630.0 °C Show Material materials with Schmelzpunkt of 630.0 °C | H36 | ||||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H36 | |||
Wärmeleitfähigkeit | 190.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 190.0 W/(m·K) | H36 | |||
193 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 193 W/(m·K) | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Elektrisch
Property | Value | Condition | Related Standards |
---|---|---|---|
Elektrische Leitfähigkeit | 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 29000000.0 S/m | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
spezifischer Widerstand | 3.45e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.45e-08 Ω·m | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 96.3 - 98.9 % Show Material materials with Aluminium of 96.3 - 98.9 % | H36 | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | H36 | |
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Eisen | 0.70 % Show Material materials with Eisen of 0.70 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
0.7 % Show Material materials with Eisen of 0.7 % | H36 | ||
Kupfer | 0.2 % Show Material materials with Kupfer of 0.2 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Magnesium | 1.1 - 1.8 % Show Material materials with Magnesium of 1.1 - 1.8 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H36 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 |
Technological properties
Property | ||
---|---|---|
Brazing | general: Lötbar mit speziellen Techniken oder bei bestimmten Anwendungen | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O), poor (H32, H34), sufficient (H36, H38) | |