Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H32 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Dehnung | 6.0 % Show Material materials with Dehnung of 6.0 % | H32 | AA Standards, ASTM B209, ASTM B313 | A50 |
8.0 % Show Material materials with Dehnung of 8.0 % | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | A50 | |
8.8 % Show Material materials with Dehnung of 8.8 % | H32 | |||
10.0 % Show Material materials with Dehnung of 10.0 % | H32 | AA Standards, ASTM B209 | A100 | |
12.0 % Show Material materials with Dehnung of 12.0 % | H32 | AA Standards, ASTM B209, ASTM B547 | A50 | |
Elastizitätsmodul | 71.0 GPa Show Material materials with Elastizitätsmodul of 71.0 GPa | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 5000 Series Aluminium | ||
Streckgrenze | 195.0 MPa Show Material materials with Streckgrenze of 195.0 MPa | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 | RP02 |
205.0 MPa Show Material materials with Streckgrenze of 205.0 MPa | H32 | AA Standards | RP02 | |
220.0 MPa Show Material materials with Streckgrenze of 220.0 MPa | H32 | |||
Zugfestigkeit | 275.0 - 325.0 MPa Show Material materials with Zugfestigkeit of 275.0 - 325.0 MPa | H32 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
275.0 MPa Show Material materials with Zugfestigkeit of 275.0 MPa | H32 | AA Standards, ASTM B210 | ||
290.0 MPa Show Material materials with Zugfestigkeit of 290.0 MPa | H32 | AA Standards | ||
300.0 MPa Show Material materials with Zugfestigkeit of 300.0 MPa | H32 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | H32 | |||
20 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 | ||
100 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||
Schmelzpunkt | 585.0 - 640.0 °C Show Material materials with Schmelzpunkt of 585.0 - 640.0 °C | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 | ||
590.0 °C Show Material materials with Schmelzpunkt of 590.0 °C | H32 | ||||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H32 | |||
Wärmeleitfähigkeit | 126 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 126 W/(m·K) | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 | ||
130.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 W/(m·K) | H32 |
Elektrisch
Property | Value | Condition | Related Standards |
---|---|---|---|
Elektrische Leitfähigkeit | 18000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 S/m | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
spezifischer Widerstand | 5.56e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.56e-08 Ω·m | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 93.0 - 96.3 % Show Material materials with Aluminium of 93.0 - 96.3 % | H32 | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | H32 | |
Chrom | 0.05 - 0.25 % Show Material materials with Chrom of 0.05 - 0.25 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Eisen | 0.50 % Show Material materials with Eisen of 0.50 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
0.5 % Show Material materials with Eisen of 0.5 % | H32 | ||
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Magnesium | 3.5 - 4.5 % Show Material materials with Magnesium of 3.5 - 4.5 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Mangan | 0.2 - 0.7 % Show Material materials with Mangan of 0.2 - 0.7 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H32 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B547 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests (O, H32, H116, H111), no damage during operation, limited damage during laboratory tests (H34, H36, H38), general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O, H32, H116, H111), sufficient (H34, H36, H38) | |
Workability | general (condition): good (O), acceptable (H32, H116, H111), poor(H36, H38) |