Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 12 % Show Material materials with Dehnung of 12 % |
Dehnung A50 | 20.0 °C | 5 - 15 % Show Material materials with Dehnung A50 of 5 - 15 % |
Elastizitätsmodul | 20.0 °C | 70 GPa Show Material materials with Elastizitätsmodul of 70 GPa |
Härte, Brinell | 20.0 °C | 67 [-] Show Material materials with Härte, Brinell of 67 [-] |
Streckgrenze | 20.0 °C | 200 MPa Show Material materials with Streckgrenze of 200 MPa |
Streckgrenze Rp 0,2 | 20.0 °C | 180 - 205 MPa Show Material materials with Streckgrenze Rp 0,2 of 180 - 205 MPa |
Zugfestigkeit | 20.0 °C | 250 - 270 MPa Show Material materials with Zugfestigkeit of 250 - 270 MPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Koeffizient der thermischen Ausdehnung | 20.0 °C | 2.4E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4E-5 1/K |
Schmelzpunkt | 590 °C Show Material materials with Schmelzpunkt of 590 °C | |
Spezifische Wärmekapazität | 20.0 °C | 900 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900 J/(kg·K) |
Wärmeleitfähigkeit | 20.0 °C | 130 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Aluminium | 94.4 - 96.8 % Show Material materials with Aluminium of 94.4 - 96.8 % |
Andere | 0.15 % Show Material materials with Andere of 0.15 % |
Chrom | 0.15 - 0.35 % Show Material materials with Chrom of 0.15 - 0.35 % |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % |
Magnesium | 3.1 - 3.9 % Show Material materials with Magnesium of 3.1 - 3.9 % |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % |
Titan | 0.2 % Show Material materials with Titan of 0.2 % |
Zink | 0.2 % Show Material materials with Zink of 0.2 % |