Allgemein
Property | Value | Condition |
---|---|---|
Dichte | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H112 |
2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H112 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Dehnung | 8.0 % Show Material materials with Dehnung of 8.0 % | H112 | AA Standards, ASTM B209, ASTM B547 | A50 |
9.0 % Show Material materials with Dehnung of 9.0 % | H112 | AA Standards, ASTM B209 | A100 | |
10.0 % Show Material materials with Dehnung of 10.0 % | H112 | AA Standards, ASTM B221, ASTM B241 | A100 | |
12.0 % Show Material materials with Dehnung of 12.0 % | H112 | AA Standards, ASTM B221, ASTM B241 | A50 | |
13.0 % Show Material materials with Dehnung of 13.0 % | H112 | AA Standards, ASTM B209 | A100 | |
14.0 % Show Material materials with Dehnung of 14.0 % | H112 | |||
18.0 % Show Material materials with Dehnung of 18.0 % | H112 | AA Standards | A50 | |
18 % Show Material materials with Dehnung of 18 % | H112 | |||
Elastizitätsmodul | 70 GPa Show Material materials with Elastizitätsmodul of 70 GPa | H112 | ||
71.0 GPa Show Material materials with Elastizitätsmodul of 71.0 GPa | H112 | |||
Härte, Brinell | 62.0 [-] Show Material materials with Härte, Brinell of 62.0 [-] | H112 | AA Standards | |
62.0 [-] Show Material materials with Härte, Brinell of 62.0 [-] | H112 | 500 kg load, 10 mm ball | ||
Kompressionsmodul | 71.0 MPa Show Material materials with Kompressionsmodul of 71.0 MPa | H112 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||
Scherfestigkeit | 159.0 MPa Show Material materials with Scherfestigkeit of 159.0 MPa | H112 | ||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 5000 Series Aluminium | ||
Streckgrenze | 85.0 MPa Show Material materials with Streckgrenze of 85.0 MPa | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241 | RP02 |
110.0 MPa Show Material materials with Streckgrenze of 110.0 MPa | H112 | |||
125.0 MPa Show Material materials with Streckgrenze of 125.0 MPa | H112 | AA Standards, ASTM B209, ASTM B547 | RP02 | |
125 MPa Show Material materials with Streckgrenze of 125 MPa | H112 | RP02 | ||
Zugfestigkeit | 215.0 MPa Show Material materials with Zugfestigkeit of 215.0 MPa | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241 | |
220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | H112 | AA Standards, ASTM B209, ASTM B547 | ||
250.0 MPa Show Material materials with Zugfestigkeit of 250.0 MPa | H112 | AA Standards | ||
250 MPa Show Material materials with Zugfestigkeit of 250 MPa | H112 |
Thermisch
Property | Value | Condition | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | H112 | |
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |
Schmelzpunkt | 600.0 °C Show Material materials with Schmelzpunkt of 600.0 °C | H112 | |
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H112 | |
Wärmeleitfähigkeit | 130.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 W/(m·K) | H112 |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 31000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 31000000.0 S/m | Typical for Wrought 5000 Series Aluminium |
spezifischer Widerstand | 3.3e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 94.5 - 97.1 % Show Material materials with Aluminium of 94.5 - 97.1 % | H112 | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | H112 | |
Chrom | 0.05 - 0.2 % Show Material materials with Chrom of 0.05 - 0.2 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Eisen | 0.40 % Show Material materials with Eisen of 0.40 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
0.4 % Show Material materials with Eisen of 0.4 % | H112 | ||
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Magnesium | 2.4 - 3.0 % Show Material materials with Magnesium of 2.4 - 3.0 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Mangan | 0.5 - 1.0 % Show Material materials with Mangan of 0.5 - 1.0 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Titan | 0.2 % Show Material materials with Titan of 0.2 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H112 | AA Standards, ASTM B209, ASTM B221, ASTM B241, ASTM B547 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O, H32, H111), sufficient (H34) | |
Workability | general (condition): good (O), acceptable (H32, H34, H111) |