Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | T1 | AA Standards, ASTM B221 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Dehnung | 14.0 % Show Material materials with Dehnung of 14.0 % | T1 | AA Standards, ASTM B221 | A100 |
16.0 % Show Material materials with Dehnung of 16.0 % | T1 | AA Standards, ASTM B221 | A50 | |
16.0 % Show Material materials with Dehnung of 16.0 % | T1 | |||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | T1 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||
Streckgrenze | 105.0 MPa Show Material materials with Streckgrenze of 105.0 MPa | T1 | AA Standards, ASTM B221 | RP02 |
120.0 MPa Show Material materials with Streckgrenze of 120.0 MPa | T1 | |||
Zugfestigkeit | 170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | T1 | AA Standards, ASTM B221 | |
200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | T1 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T1 | ||
20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | T1 | AA Standards, ASTM B221 | |
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | T1 | AA Standards, ASTM B221 | |
Schmelzpunkt | 605.0 - 655.0 °C Show Material materials with Schmelzpunkt of 605.0 - 655.0 °C | T1 | AA Standards, ASTM B221 | |
610.0 °C Show Material materials with Schmelzpunkt of 610.0 °C | T1 | |||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | T1 | ||
Wärmeleitfähigkeit | 180.0 - 188.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 180.0 - 188.0 W/(m·K) | T1 | AA Standards, ASTM B221 | |
180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 180.0 W/(m·K) | T1 |
Elektrisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Elektrische Leitfähigkeit | 27000000.0 - 28000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 27000000.0 - 28000000.0 S/m | T1 | AA Standards, ASTM B221 | |
27000000 S/m Show Material materials with Elektrische Leitfähigkeit of 27000000 S/m | T1 | Typical value | ||
Specific Electrical conductivity | 47.0 % IACS Show Material materials with Specific Electrical conductivity of 47.0 % IACS | T1 | Typical/Derived value | |
spezifischer Widerstand | 3.57e-08 - 3.7e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.57e-08 - 3.7e-08 Ω·m | T1 | AA Standards, ASTM B221 | |
3.6499999999999996e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.6499999999999996e-08 Ω·m | T1 | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 97.5 - 99.0 % Show Material materials with Aluminium of 97.5 - 99.0 % | T1 | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T1 | |
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | T1 | AA Standards, ASTM B221 |
Eisen | 0.35 % Show Material materials with Eisen of 0.35 % | T1 | AA Standards, ASTM B221 |
0.35 % Show Material materials with Eisen of 0.35 % | T1 | ||
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | T1 | AA Standards, ASTM B221 |
Magnesium | 0.4 - 0.6 % Show Material materials with Magnesium of 0.4 - 0.6 % | T1 | AA Standards, ASTM B221 |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | T1 | AA Standards, ASTM B221 |
Silizium | 0.6 - 0.9 % Show Material materials with Silizium of 0.6 - 0.9 % | T1 | AA Standards, ASTM B221 |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | T1 | AA Standards, ASTM B221 |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | T1 | AA Standards, ASTM B221 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Workability | Excellent workability. |