Allgemein
Mechanisch
Property | Value | Condition | Comment |
---|---|---|---|
Dauerfestigkeit | 97 MPa Show Material materials with Dauerfestigkeit of 97 MPa | T4 | Min., for 5x10⁸ cycles |
Dehnung | 17.0 % Show Material materials with Dehnung of 17.0 % | T4 | |
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | T4 | |
Hardness, Rockwell Superficial 15-T | 70.0 [-] Show Material materials with Hardness, Rockwell Superficial 15-T of 70.0 [-] | T4 | |
Kompressionsmodul | 69.6 MPa Show Material materials with Kompressionsmodul of 69.6 MPa | T4 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | |
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | |
Scherfestigkeit | 152.0 MPa Show Material materials with Scherfestigkeit of 152.0 MPa | T4 | |
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | |
Streckgrenze | 100.0 MPa Show Material materials with Streckgrenze of 100.0 MPa | T4 | |
Zugfestigkeit | 210.0 MPa Show Material materials with Zugfestigkeit of 210.0 MPa | T4 |
Thermisch
Property | Value | Condition | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T4 | |
Schmelzpunkt | 610.0 °C Show Material materials with Schmelzpunkt of 610.0 °C | T4 | |
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | T4 | |
Wärmeleitfähigkeit | 170.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 - 220.0 W/(m·K) | Typical for Wrought 6000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 21000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 21000000.0 - 34000000.0 S/m | Typical for Wrought 6000 Series Aluminium |
spezifischer Widerstand | 2.9e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.9e-08 - 5e-08 Ω·m | Typical for Wrought 6000 Series Aluminium |
Chemical properties
Property | Value | Condition |
---|---|---|
Aluminium | 97.5 - 99.0 % Show Material materials with Aluminium of 97.5 - 99.0 % | T4 |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T4 |
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | T4 |
Eisen | 0.35 % Show Material materials with Eisen of 0.35 % | T4 |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | T4 |
Magnesium | 0.4 - 0.6 % Show Material materials with Magnesium of 0.4 - 0.6 % | T4 |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | T4 |
Silizium | 0.6 - 0.9 % Show Material materials with Silizium of 0.6 - 0.9 % | T4 |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | T4 |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | T4 |
Technological properties
Property | ||
---|---|---|
Workability | Excellent workability. |