Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | O | ||
2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | O | EN 573-3, EN 485-2 | Sheet |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Dehnung | 39.0 % Show Material materials with Dehnung of 39.0 % | O | |||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | O | |||
71.0 GPa Show Material materials with Elastizitätsmodul of 71.0 GPa | O | EN 573-3, EN 485-2 | Sheet | ||
Härte, Brinell | 20.0 [-] Show Material materials with Härte, Brinell of 20.0 [-] | O | EN 573-3, EN 485-2 | Sheet | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | |||
Schubmodule | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | Typical for Wrought 1000 Series Aluminium | |||
Streckgrenze | 20.0 MPa Show Material materials with Streckgrenze of 20.0 MPa | O | EN 573-3, EN 485-2 | Sheet | RP02 |
26.0 MPa Show Material materials with Streckgrenze of 26.0 MPa | O | ||||
Zugfestigkeit | 65.0 - 95.0 MPa Show Material materials with Zugfestigkeit of 65.0 - 95.0 MPa | O | EN 573-3, EN 485-2 | Sheet | |
77.0 MPa Show Material materials with Zugfestigkeit of 77.0 MPa | O |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | O | EN 573-3, EN 485-2 | Sheet | ||
Schmelzpunkt | 650.0 °C Show Material materials with Schmelzpunkt of 650.0 °C | O | EN 573-3, EN 485-2 | Sheet | ||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | O | ||||
Wärmeleitfähigkeit | 222.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 222.0 W/(m·K) | O | EN 573-3, EN 485-2 | Sheet | ||
230.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 230.0 W/(m·K) | O | |||||
20 °C | 231 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 231 W/(m·K) | O | unstated value |
Elektrisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 33000000.0 - 38000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 33000000.0 - 38000000.0 S/m | Typical for Wrought 1000 Series Aluminium | |||
spezifischer Widerstand | 2.82e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.82e-08 Ω·m | O | EN 573-3, EN 485-2 | Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Aluminium | 99.5 - 100.0 % Show Material materials with Aluminium of 99.5 - 100.0 % | O | |||
Andere | 0.03 % Show Material materials with Andere of 0.03 % | O | EN 573-3, EN 485-2 | Sheet | Each |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | O | EN 573-3, EN 485-2 | Sheet | |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | O | EN 573-3, EN 485-2 | Sheet | |
Magnesium | 0.05 % Show Material materials with Magnesium of 0.05 % | O | EN 573-3, EN 485-2 | Sheet | |
Mangan | 0.05 % Show Material materials with Mangan of 0.05 % | O | EN 573-3, EN 485-2 | Sheet | |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % | O | EN 573-3, EN 485-2 | Sheet | |
Titan | 0.03 % Show Material materials with Titan of 0.03 % | O | |||
0.05 % Show Material materials with Titan of 0.05 % | O | EN 573-3, EN 485-2 | Sheet | ||
Vanadium | 0.05 % Show Material materials with Vanadium of 0.05 % | O | |||
Zink | 0.05 % Show Material materials with Zink of 0.05 % | O | |||
0.07 % Show Material materials with Zink of 0.07 % | O | EN 573-3, EN 485-2 | Sheet |
Technological properties
Property | ||
---|---|---|
Application areas | Chemical process plant equipment, Food industry containers, Pyrotechnic powder, Architectural flashings, Lamp reflectors, Cable sheathing | |
Brazing | Excellent | |
General machinability | Poor | |
Soldering general | Excellent | |
Welding | When welding 1050 to itself or an alloy from the same subgroup the recommended filler wire is 1100. For welding to alloys 5083 and 5086 or alloys from the 7XXX series, the recommend wire is 5356. For other alloys use 4043 filler wire. Gas: Excellent; Arc: Excellent; Resistance: Excellent | |
Workability | Cold: Excellent |