Allgemein
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 95.0 MPa Show Material materials with Bending Fatigue Strength of 95.0 MPa | T4 | AA Standards | |
Dehnung | 10.0 % Show Material materials with Dehnung of 10.0 % | T4 | AA Standards, ASTM B209 | A50 |
12.0 % Show Material materials with Dehnung of 12.0 % | T4 | AA Standards, ASTM B209 | A50 | |
14.0 % Show Material materials with Dehnung of 14.0 % | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B483 | A50 | |
14.0 % Show Material materials with Dehnung of 14.0 % | T4 | AA Standards, ASTM B221, ASTM B234, ASTM B241, ASTM B345 | A100 | |
16.0 % Show Material materials with Dehnung of 16.0 % | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 | A50 | |
16.0 % Show Material materials with Dehnung of 16.0 % | T4 | AA Standards, ASTM B210, ASTM B211, ASTM B234, ASTM B483 | A100 | |
18.0 % Show Material materials with Dehnung of 18.0 % | T4 | AA Standards, ASTM B210, ASTM B211, ASTM B234, ASTM B483 | A50 | |
19.0 % Show Material materials with Dehnung of 19.0 % | T4 | |||
22.0 % Show Material materials with Dehnung of 22.0 % | T4 | AA Standards | A50 | |
22.0 % Show Material materials with Dehnung of 22.0 % | T4 | AA Standards | A100 | |
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 | |
Härte, Brinell | 65.0 [-] Show Material materials with Härte, Brinell of 65.0 [-] | T4 | AA Standards | |
65.0 [-] Show Material materials with Härte, Brinell of 65.0 [-] | T4 | 500 kg load, 10 mm ball | ||
Kompressionsmodul | 69.7 MPa Show Material materials with Kompressionsmodul of 69.7 MPa | T4 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||
Scherfestigkeit | 165.0 MPa Show Material materials with Scherfestigkeit of 165.0 MPa | T4 | ||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||
Streckgrenze | 100.0 MPa Show Material materials with Streckgrenze of 100.0 MPa | T4 | AA Standards, ASTM B210 | RP02 |
110.0 MPa Show Material materials with Streckgrenze of 110.0 MPa | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 | RP02 | |
130.0 MPa Show Material materials with Streckgrenze of 130.0 MPa | T4 | |||
145.0 MPa Show Material materials with Streckgrenze of 145.0 MPa | T4 | AA Standards | RP02 | |
145 MPa Show Material materials with Streckgrenze of 145 MPa | T4 | RP02 | ||
Zugfestigkeit | 180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | T4 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | |
205.0 MPa Show Material materials with Zugfestigkeit of 205.0 MPa | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B234, ASTM B313, ASTM B483, ASTM B547 | ||
230.0 MPa Show Material materials with Zugfestigkeit of 230.0 MPa | T4 | |||
240.0 MPa Show Material materials with Zugfestigkeit of 240.0 MPa | T4 | AA Standards | ||
240 MPa Show Material materials with Zugfestigkeit of 240 MPa | T4 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | T4 | ||
20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 | |
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 | |
Schmelzpunkt | 580.0 - 650.0 °C Show Material materials with Schmelzpunkt of 580.0 - 650.0 °C | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 | |
580.0 °C Show Material materials with Schmelzpunkt of 580.0 °C | T4 | |||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | T4 | ||
Wärmeleitfähigkeit | 155.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 155.0 - 180.0 W/(m·K) | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 | |
170.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 W/(m·K) | T4 |
Elektrisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Elektrische Leitfähigkeit | 23000000.0 - 27000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 27000000.0 S/m | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 | |
23000000 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000 S/m | T4 | Typical value | ||
Specific Electrical conductivity | 40.0 % IACS Show Material materials with Specific Electrical conductivity of 40.0 % IACS | T4 | Typical/Derived value | |
spezifischer Widerstand | 3.7e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.7e-08 - 4.35e-08 Ω·m | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 | |
4.3e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.3e-08 Ω·m | T4 | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 95.9 - 98.6 % Show Material materials with Aluminium of 95.9 - 98.6 % | T4 | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T4 | |
Chrom | 0.04 - 0.35 % Show Material materials with Chrom of 0.04 - 0.35 % | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 |
Eisen | 0.70 % Show Material materials with Eisen of 0.70 % | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 |
0.7 % Show Material materials with Eisen of 0.7 % | T4 | ||
Kupfer | 0.15 - 0.4 % Show Material materials with Kupfer of 0.15 - 0.4 % | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 |
Magnesium | 0.8 - 1.2 % Show Material materials with Magnesium of 0.8 - 1.2 % | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 |
Mangan | 0.15 % Show Material materials with Mangan of 0.15 % | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 |
Silizium | 0.4 - 0.8 % Show Material materials with Silizium of 0.4 - 0.8 % | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | T4 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B221, ASTM B234, ASTM B241, ASTM B313, ASTM B345, ASTM B483, ASTM B547 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests (O, T6, T651, T652, T6510, T6511), no damage during operation, limited damage during laboratory tests (T4, T451, T4510, T4511), general: good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O), sufficient (T4, T451, T4510, T4511, T6, T651, T652, T6510, T6511) | |
Workability | general (condition): good (O), acceptable (T4, T451, T4510, T4511), poor(T6, T651, T652, T6510, T6511) |