Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | T6511 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | Bar, Tube, Sheet |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Dehnung | 8.0 % Show Material materials with Dehnung of 8.0 % | T6511 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | A50 | |
8.0 - 10.0 % Show Material materials with Dehnung of 8.0 - 10.0 % | T6511 | Bar, Tube, Sheet | |||
9.0 % Show Material materials with Dehnung of 9.0 % | T6511 | AA Standards, ASTM B221, ASTM B241 | A100 | ||
9.2 % Show Material materials with Dehnung of 9.2 % | T6511 | ||||
10.0 % Show Material materials with Dehnung of 10.0 % | T6511 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | A50 | ||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | T6511 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | ||
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | T6511 | Bar, Tube, Sheet | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | |||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | |||
Streckgrenze | 240.0 MPa Show Material materials with Streckgrenze of 240.0 MPa | T6511 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | RP02 | |
262.0 MPa Show Material materials with Streckgrenze of 262.0 MPa | T6511 | Bar, Tube, Sheet | RP02 | ||
280.0 MPa Show Material materials with Streckgrenze of 280.0 MPa | T6511 | ||||
Zugfestigkeit | 241.0 MPa Show Material materials with Zugfestigkeit of 241.0 MPa | T6511 | Bar, Tube, Sheet | ||
260.0 MPa Show Material materials with Zugfestigkeit of 260.0 MPa | T6511 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | |||
300.0 MPa Show Material materials with Zugfestigkeit of 300.0 MPa | T6511 |
Thermisch
Property | Temperature | Value | Condition | Shape | Related Standards |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.34e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.34e-05 1/K | T6511 | Bar, Tube, Sheet | ||
2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | T6511 | ||||
20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | T6511 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | ||
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | T6511 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | ||
Schmelzpunkt | 580.0 - 650.0 °C Show Material materials with Schmelzpunkt of 580.0 - 650.0 °C | T6511 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | ||
580.0 °C Show Material materials with Schmelzpunkt of 580.0 °C | T6511 | ||||
650.0 °C Show Material materials with Schmelzpunkt of 650.0 °C | T6511 | Bar, Tube, Sheet | |||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | T6511 | |||
Wärmeleitfähigkeit | 155.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 155.0 - 180.0 W/(m·K) | T6511 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | ||
166.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 166.0 W/(m·K) | T6511 | Bar, Tube, Sheet | |||
170.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 W/(m·K) | T6511 |
Elektrisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Elektrische Leitfähigkeit | 23000000.0 - 27000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 27000000.0 S/m | T6511 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | |
spezifischer Widerstand | 3.7e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.7e-08 - 4.35e-08 Ω·m | T6511 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | |
4e-08 Ω·m Show Material materials with spezifischer Widerstand of 4e-08 Ω·m | T6511 | Bar, Tube, Sheet |
Chemical properties
Property | Value | Condition | Shape | Related Standards | Comment |
---|---|---|---|---|---|
Aluminium | 95.9 - 98.6 % Show Material materials with Aluminium of 95.9 - 98.6 % | T6511 | |||
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T6511 | Bar, Tube, Sheet | Total | |
Chrom | 0.04 - 0.35 % Show Material materials with Chrom of 0.04 - 0.35 % | T6511 | Bar, Tube, Sheet | AA Standards, ASTM B221, ASTM B241, ASTM B345 | |
Eisen | 0.70 % Show Material materials with Eisen of 0.70 % | T6511 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | ||
0.7 % Show Material materials with Eisen of 0.7 % | T6511 | Bar, Tube, Sheet | |||
Kupfer | 0.15 - 0.4 % Show Material materials with Kupfer of 0.15 - 0.4 % | T6511 | Bar, Tube, Sheet | AA Standards, ASTM B221, ASTM B241, ASTM B345 | |
Magnesium | 0.8 - 1.2 % Show Material materials with Magnesium of 0.8 - 1.2 % | T6511 | Bar, Tube, Sheet | AA Standards, ASTM B221, ASTM B241, ASTM B345 | |
Mangan | 0.15 % Show Material materials with Mangan of 0.15 % | T6511 | Bar, Tube, Sheet | AA Standards, ASTM B221, ASTM B241, ASTM B345 | |
Silizium | 0.4 - 0.8 % Show Material materials with Silizium of 0.4 - 0.8 % | T6511 | Bar, Tube, Sheet | AA Standards, ASTM B221, ASTM B241, ASTM B345 | |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | T6511 | Bar, Tube, Sheet | AA Standards, ASTM B221, ASTM B241, ASTM B345 | |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | T6511 | Bar, Tube, Sheet | AA Standards, ASTM B221, ASTM B241, ASTM B345 |
Technological properties
Property | ||
---|---|---|
Application areas | Aerospace | |
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests (O, T6, T651, T652, T6510, T6511), no damage during operation, limited damage during laboratory tests (T4, T451, T4510, T4511), general: good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (O), sufficient (T4, T451, T4510, T4511, T6, T651, T652, T6510, T6511) | |
Workability | general (condition): good (O), acceptable (T4, T451, T4510, T4511), poor(T6, T651, T652, T6510, T6511) |