Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube |
2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | O |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 55.0 MPa Show Material materials with Bending Fatigue Strength of 55.0 MPa | O | AA Standards | ||
Dauerfestigkeit | 55 MPa Show Material materials with Dauerfestigkeit of 55 MPa | O | fo 5x10⁸ cycles | ||
Dehnung | 16.0 % Show Material materials with Dehnung of 16.0 % | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | A50 |
16.0 % Show Material materials with Dehnung of 16.0 % | O | AA Standards, ASTM B221, ASTM B241, ASTM B345 | A100 | ||
18.0 % Show Material materials with Dehnung of 18.0 % | O | AA Standards, ASTM B221, ASTM B241, ASTM B345 | A50 | ||
18.0 % Show Material materials with Dehnung of 18.0 % | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
22.0 % Show Material materials with Dehnung of 22.0 % | O | ||||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||
69 GPa Show Material materials with Elastizitätsmodul of 69 GPa | O | ||||
69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
Härte, Brinell | 25.0 [-] Show Material materials with Härte, Brinell of 25.0 [-] | O | AA Standards, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
25.0 [-] Show Material materials with Härte, Brinell of 25.0 [-] | O | 500 kg load, 10 mm ball | |||
Kompressionsmodul | 69.7 MPa Show Material materials with Kompressionsmodul of 69.7 MPa | O | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | |||
Scherfestigkeit | 69.0 MPa Show Material materials with Scherfestigkeit of 69.0 MPa | O | |||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | |||
Streckgrenze | 49.0 MPa Show Material materials with Streckgrenze of 49.0 MPa | O | |||
50.0 MPa Show Material materials with Streckgrenze of 50.0 MPa | O | AA Standards | RP02 | ||
50 MPa Show Material materials with Streckgrenze of 50 MPa | O | RP02 | |||
Zugfestigkeit | 90.0 MPa Show Material materials with Zugfestigkeit of 90.0 MPa | O | AA Standards | ||
90 MPa Show Material materials with Zugfestigkeit of 90 MPa | O | ||||
110.0 MPa Show Material materials with Zugfestigkeit of 110.0 MPa | O | ||||
130.0 MPa Show Material materials with Zugfestigkeit of 130.0 MPa | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | O | ||||
2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |||
20 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |||
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |||
Schmelzpunkt | 600.0 °C Show Material materials with Schmelzpunkt of 600.0 °C | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
615.0 - 655.0 °C Show Material materials with Schmelzpunkt of 615.0 - 655.0 °C | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||||
620.0 °C Show Material materials with Schmelzpunkt of 620.0 °C | O | |||||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | O | ||||
Wärmeleitfähigkeit | 193.0 - 218.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 193.0 - 218.0 W/(m·K) | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |||
200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 200.0 W/(m·K) | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |||
25 °C | 218 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 218 W/(m·K) | O | unstated value |
Elektrisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 29000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 29000000.0 - 34000000.0 S/m | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||
34000000 S/m Show Material materials with Elektrische Leitfähigkeit of 34000000 S/m | O | Typical value | |||
Specific Electrical conductivity | 59.0 % IACS Show Material materials with Specific Electrical conductivity of 59.0 % IACS | O | Typical/Derived value | ||
spezifischer Widerstand | 2.9e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.9e-08 Ω·m | O | Typical value | ||
2.94e-08 - 3.45e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.94e-08 - 3.45e-08 Ω·m | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |||
3.5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.5e-08 Ω·m | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Aluminium | 97.5 - 99.4 % Show Material materials with Aluminium of 97.5 - 99.4 % | O | |||
Andere | 0.15 % Show Material materials with Andere of 0.15 % | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | Total |
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Eisen | 0.35 % Show Material materials with Eisen of 0.35 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||
0.35 % Show Material materials with Eisen of 0.35 % | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Magnesium | 0.45 - 0.9 % Show Material materials with Magnesium of 0.45 - 0.9 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Silizium | 0.2 - 0.6 % Show Material materials with Silizium of 0.2 - 0.6 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube |
Technological properties
Property | ||
---|---|---|
Application areas | - 6063 Architectural, applications, Extrusions, Window frames, Doors, Shop fittings, Irrigation tubing, In balustrading the rails and posts are normally in the T6 temper and formed elbows and bends are T4. T4 temper 6063 aluminium is also finding applications in hydroformed tube for chassis. - 6063A 6063A is used in the same applications as 6063. It is also used in: Road transport Rail transport Extreme sports equipment | |
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (T1, T4), sufficient (T5, T452, T6, T83, T831, T832) | |
Soldering general | Good | |
Welding | 6063 is suitable for all conventional welding methods. Welding wire generally should be alloy 5183 or alloy 4043. When maximum electrical conductivity is required use alloy 4043. For strength and conductivity use alloy 5346 and increase the size of the weld to compensate for the lower conductivity. Gas: Excellent; Arc:Excellent; Resistance:Excellent. | |
Workability | general (condition): acceptable (T1, T4, T5, T452), poor(T6, T83, T831, T832) |