Allgemein
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Dehnung | 12.0 % Show Material materials with Dehnung of 12.0 % | T4 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | A100 |
14.0 % Show Material materials with Dehnung of 14.0 % | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | A50 | |
16.0 % Show Material materials with Dehnung of 16.0 % | T4 | AA Standards, ASTM B210, ASTM B483 | A50 | |
16.0 % Show Material materials with Dehnung of 16.0 % | T4 | AA Standards, ASTM B210, ASTM B483 | A100 | |
17.0 % Show Material materials with Dehnung of 17.0 % | T4 | |||
18.0 % Show Material materials with Dehnung of 18.0 % | T4 | AA Standards, ASTM B210, ASTM B483 | A50 | |
22.0 % Show Material materials with Dehnung of 22.0 % | T4 | AA Standards | A50 | |
22 % Show Material materials with Dehnung of 22 % | T4 | |||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |
69 GPa Show Material materials with Elastizitätsmodul of 69 GPa | T4 | |||
Kompressionsmodul | 69.7 MPa Show Material materials with Kompressionsmodul of 69.7 MPa | T4 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||
Streckgrenze | 60.0 MPa Show Material materials with Streckgrenze of 60.0 MPa | T4 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | RP02 |
70.0 MPa Show Material materials with Streckgrenze of 70.0 MPa | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | RP02 | |
83.0 MPa Show Material materials with Streckgrenze of 83.0 MPa | T4 | |||
90.0 MPa Show Material materials with Streckgrenze of 90.0 MPa | T4 | AA Standards | RP02 | |
90 MPa Show Material materials with Streckgrenze of 90 MPa | T4 | RP02 | ||
Zugfestigkeit | 125.0 MPa Show Material materials with Zugfestigkeit of 125.0 MPa | T4 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | |
130.0 MPa Show Material materials with Zugfestigkeit of 130.0 MPa | T4 | AA Standards, ASTM B221, ASTM B241, ASTM B345 | ||
150.0 MPa Show Material materials with Zugfestigkeit of 150.0 MPa | T4 | AA Standards, ASTM B210, ASTM B483 | ||
160.0 MPa Show Material materials with Zugfestigkeit of 160.0 MPa | T4 | |||
170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | T4 | AA Standards | ||
170 MPa Show Material materials with Zugfestigkeit of 170 MPa | T4 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T4 | ||
20 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |
Schmelzpunkt | 615.0 - 655.0 °C Show Material materials with Schmelzpunkt of 615.0 - 655.0 °C | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |
620.0 °C Show Material materials with Schmelzpunkt of 620.0 °C | T4 | |||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | T4 | ||
Wärmeleitfähigkeit | 193.0 - 218.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 193.0 - 218.0 W/(m·K) | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |
200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 200.0 W/(m·K) | T4 |
Elektrisch
Property | Value | Condition | Related Standards |
---|---|---|---|
Elektrische Leitfähigkeit | 29000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 29000000.0 - 34000000.0 S/m | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
spezifischer Widerstand | 2.94e-08 - 3.45e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.94e-08 - 3.45e-08 Ω·m | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 97.5 - 99.4 % Show Material materials with Aluminium of 97.5 - 99.4 % | T4 | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T4 | |
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Eisen | 0.35 % Show Material materials with Eisen of 0.35 % | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
0.35 % Show Material materials with Eisen of 0.35 % | T4 | ||
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Magnesium | 0.45 - 0.9 % Show Material materials with Magnesium of 0.45 - 0.9 % | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Silizium | 0.2 - 0.6 % Show Material materials with Silizium of 0.2 - 0.6 % | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | T4 | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (T1, T4), sufficient (T5, T452, T6, T83, T831, T832) | |
Workability | general (condition): acceptable (T1, T4, T5, T452), poor(T6, T83, T831, T832) |