Allgemein
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Dehnung | 7.4 % Show Material materials with Dehnung of 7.4 % | T83 | ||
9 % Show Material materials with Dehnung of 9 % | T83 | |||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | T83 | AA Standards, ASTM B210, ASTM B483 | |
69 GPa Show Material materials with Elastizitätsmodul of 69 GPa | T83 | |||
Härte, Brinell | 82.0 [-] Show Material materials with Härte, Brinell of 82.0 [-] | T83 | 500 kg load, 10 mm ball | |
Kompressionsmodul | 69.7 MPa Show Material materials with Kompressionsmodul of 69.7 MPa | T83 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||
Scherfestigkeit | 152.0 MPa Show Material materials with Scherfestigkeit of 152.0 MPa | T83 | ||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||
Streckgrenze | 205.0 MPa Show Material materials with Streckgrenze of 205.0 MPa | T83 | AA Standards, ASTM B210, ASTM B483 | RP02 |
240 MPa Show Material materials with Streckgrenze of 240 MPa | T83 | RP02 | ||
240.0 MPa Show Material materials with Streckgrenze of 240.0 MPa | T83 | |||
Zugfestigkeit | 230.0 MPa Show Material materials with Zugfestigkeit of 230.0 MPa | T83 | AA Standards, ASTM B210, ASTM B483 | |
255 MPa Show Material materials with Zugfestigkeit of 255 MPa | T83 | |||
260.0 MPa Show Material materials with Zugfestigkeit of 260.0 MPa | T83 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T83 | ||
20 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T83 | AA Standards, ASTM B210, ASTM B483 | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T83 | AA Standards, ASTM B210, ASTM B483 | |
Schmelzpunkt | 615.0 - 655.0 °C Show Material materials with Schmelzpunkt of 615.0 - 655.0 °C | T83 | AA Standards, ASTM B210, ASTM B483 | |
620.0 °C Show Material materials with Schmelzpunkt of 620.0 °C | T83 | |||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | T83 | ||
Wärmeleitfähigkeit | 193.0 - 218.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 193.0 - 218.0 W/(m·K) | T83 | AA Standards, ASTM B210, ASTM B483 | |
200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 200.0 W/(m·K) | T83 |
Elektrisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Elektrische Leitfähigkeit | 29000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 29000000.0 - 34000000.0 S/m | T83 | AA Standards, ASTM B210, ASTM B483 | |
31000000 S/m Show Material materials with Elektrische Leitfähigkeit of 31000000 S/m | T83 | Typical value | ||
Specific Electrical conductivity | 53.0 % IACS Show Material materials with Specific Electrical conductivity of 53.0 % IACS | T83 | Typical/Derived value | |
spezifischer Widerstand | 2.94e-08 - 3.45e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.94e-08 - 3.45e-08 Ω·m | T83 | AA Standards, ASTM B210, ASTM B483 | |
3.2e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.2e-08 Ω·m | T83 | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 97.5 - 99.4 % Show Material materials with Aluminium of 97.5 - 99.4 % | T83 | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | T83 | |
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | T83 | AA Standards, ASTM B210, ASTM B483 |
Eisen | 0.35 % Show Material materials with Eisen of 0.35 % | T83 | AA Standards, ASTM B210, ASTM B483 |
0.35 % Show Material materials with Eisen of 0.35 % | T83 | ||
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | T83 | AA Standards, ASTM B210, ASTM B483 |
Magnesium | 0.45 - 0.9 % Show Material materials with Magnesium of 0.45 - 0.9 % | T83 | AA Standards, ASTM B210, ASTM B483 |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | T83 | AA Standards, ASTM B210, ASTM B483 |
Silizium | 0.2 - 0.6 % Show Material materials with Silizium of 0.2 - 0.6 % | T83 | AA Standards, ASTM B210, ASTM B483 |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | T83 | AA Standards, ASTM B210, ASTM B483 |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | T83 | AA Standards, ASTM B210, ASTM B483 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (T1, T4), sufficient (T5, T452, T6, T83, T831, T832) | |
Workability | general (condition): acceptable (T1, T4, T5, T452), poor(T6, T83, T831, T832) |