Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H12 | |
2.705 g/cm³ Show Material materials with Dichte of 2.705 g/cm³ | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 30.0 MPa Show Material materials with Bending Fatigue Strength of 30.0 MPa | H12 | AA Standards | |
Dauerfestigkeit | 28 MPa Show Material materials with Dauerfestigkeit of 28 MPa | H12 | for 5x10⁸ cycles | |
Dehnung | 6.0 % Show Material materials with Dehnung of 6.0 % | H12 | AA Standards, ASTM B209 | A50 |
7.0 % Show Material materials with Dehnung of 7.0 % | H12 | AA Standards, ASTM B209 | A50 | |
10.0 % Show Material materials with Dehnung of 10.0 % | H12 | AA Standards, ASTM B209 | A100 | |
12.0 % Show Material materials with Dehnung of 12.0 % | H12 | AA Standards, ASTM B209 | A50 | |
12.0 % Show Material materials with Dehnung of 12.0 % | H12 | |||
16.0 % Show Material materials with Dehnung of 16.0 % | H12 | AA Standards | A50 | |
16 % Show Material materials with Dehnung of 16 % | H12 | |||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 | |
69 GPa Show Material materials with Elastizitätsmodul of 69 GPa | H12 | |||
Härte, Brinell | 23.0 [-] Show Material materials with Härte, Brinell of 23.0 [-] | H12 | AA Standards | |
28.0 [-] Show Material materials with Härte, Brinell of 28.0 [-] | H12 | 500 kg load, 10 mm ball | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||
Scherfestigkeit | 55.0 MPa Show Material materials with Scherfestigkeit of 55.0 MPa | H12 | ||
Schubmodule | 25.0 GPa Show Material materials with Schubmodule of 25.0 GPa | H12 | ||
Streckgrenze | 30.0 MPa Show Material materials with Streckgrenze of 30.0 MPa | H12 | AA Standards, ASTM B210, ASTM B483 | RP02 |
60.0 MPa Show Material materials with Streckgrenze of 60.0 MPa | H12 | AA Standards, ASTM B209 | RP02 | |
62.0 MPa Show Material materials with Streckgrenze of 62.0 MPa | H12 | |||
75.0 MPa Show Material materials with Streckgrenze of 75.0 MPa | H12 | AA Standards | RP02 | |
75 MPa Show Material materials with Streckgrenze of 75 MPa | H12 | RP02 | ||
Zugfestigkeit | 70.0 MPa Show Material materials with Zugfestigkeit of 70.0 MPa | H12 | AA Standards, ASTM B210, ASTM B483 | |
75.0 - 110.0 MPa Show Material materials with Zugfestigkeit of 75.0 - 110.0 MPa | H12 | AA Standards, ASTM B209 | ||
85.0 MPa Show Material materials with Zugfestigkeit of 85.0 MPa | H12 | AA Standards | ||
85 MPa Show Material materials with Zugfestigkeit of 85 MPa | H12 | |||
86.0 MPa Show Material materials with Zugfestigkeit of 86.0 MPa | H12 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | H12 | ||
20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 | |
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 | |
Schmelzpunkt | 645.0 - 655.0 °C Show Material materials with Schmelzpunkt of 645.0 - 655.0 °C | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 | |
650.0 °C Show Material materials with Schmelzpunkt of 650.0 °C | H12 | |||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H12 | ||
Wärmeleitfähigkeit | 230.0 - 234.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 230.0 - 234.0 W/(m·K) | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 | |
230.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 230.0 W/(m·K) | H12 |
Elektrisch
Property | Value | Condition | Related Standards |
---|---|---|---|
Elektrische Leitfähigkeit | 35000000.0 - 36000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 35000000.0 - 36000000.0 S/m | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 |
spezifischer Widerstand | 2.78e-08 - 2.86e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.78e-08 - 2.86e-08 Ω·m | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 99.6 % Show Material materials with Aluminium of 99.6 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 |
99.6 - 100.0 % Show Material materials with Aluminium of 99.6 - 100.0 % | H12 | ||
Eisen | 0.35 % Show Material materials with Eisen of 0.35 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 |
0.35 % Show Material materials with Eisen of 0.35 % | H12 | ||
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 |
Magnesium | 0.03 % Show Material materials with Magnesium of 0.03 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 |
Mangan | 0.03 % Show Material materials with Mangan of 0.03 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 |
Titan | 0.03 % Show Material materials with Titan of 0.03 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 |
Vanadium | 0.05 % Show Material materials with Vanadium of 0.05 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 |
Zink | 0.05 % Show Material materials with Zink of 0.05 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B483 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12), poor (H14, H16, H18) | |
Workability | general (condition): good (O, H12, H14), acceptable (H16, H18) |