Allgemein
Property | Value | Condition |
---|---|---|
Dichte | 2.78 g/cm³ Show Material materials with Dichte of 2.78 g/cm³ | O |
2.9 g/cm³ Show Material materials with Dichte of 2.9 g/cm³ | O |
Mechanisch
Property | Value | Condition | Comment |
---|---|---|---|
Dehnung | 20.0 % Show Material materials with Dehnung of 20.0 % | O | |
Elastizitätsmodul | 71.0 GPa Show Material materials with Elastizitätsmodul of 71.0 GPa | O | |
Kompressionsmodul | 72.4 MPa Show Material materials with Kompressionsmodul of 72.4 MPa | O | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium | |
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | |
Scherfestigkeit | 117.0 MPa Show Material materials with Scherfestigkeit of 117.0 MPa | O | |
Schubmodule | 26.9 GPa Show Material materials with Schubmodule of 26.9 GPa | O | |
Streckgrenze | 95.0 MPa Show Material materials with Streckgrenze of 95.0 MPa | O | |
Zugfestigkeit | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | O |
Thermisch
Property | Value | Condition |
---|---|---|
Koeffizient der thermischen Ausdehnung | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | O |
Schmelzpunkt | 610.0 °C Show Material materials with Schmelzpunkt of 610.0 °C | O |
Spezifische Wärmekapazität | 880.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 880.0 J/(kg·K) | O |
Wärmeleitfähigkeit | 170.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 W/(m·K) | O |
Elektrisch
Property | Value | Condition | Comment |
---|---|---|---|
Elektrische Leitfähigkeit | 25000000 S/m Show Material materials with Elektrische Leitfähigkeit of 25000000 S/m | O | Typical/derived value |
Specific Electrical conductivity | 43.0 % IACS Show Material materials with Specific Electrical conductivity of 43.0 % IACS | O | Typical value |
spezifischer Widerstand | 4.0099999999999995e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.0099999999999995e-08 Ω·m | O | Typical value |
Chemical properties
Property | Value | Condition |
---|---|---|
Aluminium | 91.0 - 94.7 % Show Material materials with Aluminium of 91.0 - 94.7 % | O |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | O |
Chrom | 0.06 - 0.2 % Show Material materials with Chrom of 0.06 - 0.2 % | O |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | O |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | O |
Magnesium | 1.0 - 1.8 % Show Material materials with Magnesium of 1.0 - 1.8 % | O |
Mangan | 0.2 - 0.7 % Show Material materials with Mangan of 0.2 - 0.7 % | O |
Silizium | 0.35 % Show Material materials with Silizium of 0.35 % | O |
Titan | 0.01 - 0.06 % Show Material materials with Titan of 0.01 - 0.06 % | O |
Zink | 4.0 - 5.0 % Show Material materials with Zink of 4.0 - 5.0 % | O |
Zirkonium | 0.08 - 0.2 % Show Material materials with Zirkonium of 0.08 - 0.2 % | O |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent |