Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H12 | ||
2.8 g/cm³ Show Material materials with Dichte of 2.8 g/cm³ | H12 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 40.0 MPa Show Material materials with Bending Fatigue Strength of 40.0 MPa | H12 | AA Standards | |
Dauerfestigkeit | 41 MPa Show Material materials with Dauerfestigkeit of 41 MPa | H12 | for 5x10⁸ cycles | |
Dehnung | 3.0 % Show Material materials with Dehnung of 3.0 % | H12 | AA Standards, ASTM B209 | A50 |
5.0 % Show Material materials with Dehnung of 5.0 % | H12 | AA Standards, ASTM B209, ASTM B313 | A50 | |
8.0 % Show Material materials with Dehnung of 8.0 % | H12 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | A50 | |
9.0 % Show Material materials with Dehnung of 9.0 % | H12 | AA Standards, ASTM B209 | A100 | |
10.0 % Show Material materials with Dehnung of 10.0 % | H12 | AA Standards, ASTM B209, ASTM B547 | A50 | |
12.0 % Show Material materials with Dehnung of 12.0 % | H12 | AA Standards | A50 | |
13.0 % Show Material materials with Dehnung of 13.0 % | H12 | |||
18.5 % Show Material materials with Dehnung of 18.5 % | H12 | |||
22.0 % Show Material materials with Dehnung of 22.0 % | H12 | AA Standards | A100 | |
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
69 GPa Show Material materials with Elastizitätsmodul of 69 GPa | H12 | |||
Härte, Brinell | 28.0 [-] Show Material materials with Härte, Brinell of 28.0 [-] | H12 | AA Standards | |
28.0 [-] Show Material materials with Härte, Brinell of 28.0 [-] | H12 | 500 kg load, 10 mm ball | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||
Scherfestigkeit | 70.0 MPa Show Material materials with Scherfestigkeit of 70.0 MPa | H12 | ||
Schubmodule | 25.0 GPa Show Material materials with Schubmodule of 25.0 GPa | H12 | ||
Streckgrenze | 75.0 MPa Show Material materials with Streckgrenze of 75.0 MPa | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B313, ASTM B483, ASTM B547 | RP02 |
93.0 MPa Show Material materials with Streckgrenze of 93.0 MPa | H12 | |||
105.0 MPa Show Material materials with Streckgrenze of 105.0 MPa | H12 | AA Standards | RP02 | |
105 MPa Show Material materials with Streckgrenze of 105 MPa | H12 | RP02 | ||
Zugfestigkeit | 95.0 - 130.0 MPa Show Material materials with Zugfestigkeit of 95.0 - 130.0 MPa | H12 | AA Standards, ASTM B209, ASTM B313, ASTM B547 | |
95.0 MPa Show Material materials with Zugfestigkeit of 95.0 MPa | H12 | AA Standards, ASTM B210, ASTM B211, ASTM B483 | ||
110.0 MPa Show Material materials with Zugfestigkeit of 110.0 MPa | H12 | AA Standards | ||
110 MPa Show Material materials with Zugfestigkeit of 110 MPa | H12 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | H12 | ||
20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
Schmelzpunkt | 640.0 - 655.0 °C Show Material materials with Schmelzpunkt of 640.0 - 655.0 °C | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
640.0 °C Show Material materials with Schmelzpunkt of 640.0 °C | H12 | |||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H12 | ||
Wärmeleitfähigkeit | 218.0 - 222.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 218.0 - 222.0 W/(m·K) | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 | |
220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 220.0 W/(m·K) | H12 |
Elektrisch
Property | Value | Condition | Related Standards |
---|---|---|---|
Elektrische Leitfähigkeit | 33000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 33000000.0 - 34000000.0 S/m | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
spezifischer Widerstand | 2.94e-08 - 3.03e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.94e-08 - 3.03e-08 Ω·m | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 99.0 % Show Material materials with Aluminium of 99.0 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
99.0 - 100.0 % Show Material materials with Aluminium of 99.0 - 100.0 % | H12 | ||
Andere | 0.15 % Show Material materials with Andere of 0.15 % | H12 | |
Eisen | 1.0 % Show Material materials with Eisen of 1.0 % | H12 | |
Kupfer | 0.05 - 0.2 % Show Material materials with Kupfer of 0.05 - 0.2 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Mangan | 0.05 % Show Material materials with Mangan of 0.05 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Silizium | 1.0 % Show Material materials with Silizium of 1.0 % | H12 | |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | H12 | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B313, ASTM B483, ASTM B547 |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12), poor (H14, H16, H18) | |
Workability | general (condition): good (O, H12, H14), acceptable (H16), poor(H18) |