Allgemein
Property | Value | Condition |
---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H112 |
Mechanisch
Property | Value | Condition | Comment |
---|---|---|---|
Dehnung | 29.0 % Show Material materials with Dehnung of 29.0 % | H112 | |
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H112 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | |
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | |
Schubmodule | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | Typical for Wrought 1000 Series Aluminium | |
Streckgrenze | 29.0 MPa Show Material materials with Streckgrenze of 29.0 MPa | H112 | |
Zugfestigkeit | 69.0 MPa Show Material materials with Zugfestigkeit of 69.0 MPa | H112 |
Thermisch
Property | Value | Condition |
---|---|---|
Koeffizient der thermischen Ausdehnung | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | H112 |
Schmelzpunkt | 650.0 °C Show Material materials with Schmelzpunkt of 650.0 °C | H112 |
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H112 |
Wärmeleitfähigkeit | 230.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 230.0 W/(m·K) | H112 |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 33000000.0 - 38000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 33000000.0 - 38000000.0 S/m | Typical for Wrought 1000 Series Aluminium |
spezifischer Widerstand | 2.7e-08 - 3e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.7e-08 - 3e-08 Ω·m | Typical for Wrought 1000 Series Aluminium |
Chemical properties
Property | Value | Condition |
---|---|---|
Aluminium | 99.5 - 100.0 % Show Material materials with Aluminium of 99.5 - 100.0 % | H112 |
Andere | 0.1 % Show Material materials with Andere of 0.1 % | H112 |
Bor | 0.05 % Show Material materials with Bor of 0.05 % | H112 |
Chrom | 0.01 % Show Material materials with Chrom of 0.01 % | H112 |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | H112 |
Gallium | 0.03 % Show Material materials with Gallium of 0.03 % | H112 |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | H112 |
Mangan | 0.01 % Show Material materials with Mangan of 0.01 % | H112 |
Silizium | 0.1 % Show Material materials with Silizium of 0.1 % | H112 |
Titan | 0.02 % Show Material materials with Titan of 0.02 % | H112 |
Vanadium | 0.02 % Show Material materials with Vanadium of 0.02 % | H112 |
Zink | 0.05 % Show Material materials with Zink of 0.05 % | H112 |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent | |
Workability | Excellent workability. |