Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 8.7 g/cm³ Show Material materials with Dichte of 8.7 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 23.0 °C | 34 - 35 % Show Material materials with Dehnung of 34 - 35 % |
Elastizitätsmodul | 23.0 °C | 210 GPa Show Material materials with Elastizitätsmodul of 210 GPa |
Streckgrenze | 23.0 °C | 330 - 460 MPa Show Material materials with Streckgrenze of 330 - 460 MPa |
Zugfestigkeit | 23.0 °C | 810 - 920 MPa Show Material materials with Zugfestigkeit of 810 - 920 MPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.3E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.3E-5 1/K |
Schmelzpunkt | 1290 °C Show Material materials with Schmelzpunkt of 1290 °C | |
Spezifische Wärmekapazität | 23.0 °C | 440 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 440 J/(kg·K) |
Wärmeleitfähigkeit | 23.0 °C | 12 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 12 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Aluminium | 0 - 0.4 % Show Material materials with Aluminium of 0 - 0.4 % |
Chrom | 20 - 23 % Show Material materials with Chrom of 20 - 23 % |
Eisen | 0 - 5 % Show Material materials with Eisen of 0 - 5 % |
Kobalt | 0 - 1 % Show Material materials with Kobalt of 0 - 1 % |
Kohlenstoff | 0 - 0.1 % Show Material materials with Kohlenstoff of 0 - 0.1 % |
Mangan | 0 - 0.5 % Show Material materials with Mangan of 0 - 0.5 % |
Molybdän | 8 - 10 % Show Material materials with Molybdän of 8 - 10 % |
Nickel | 58 - 68.9 % Show Material materials with Nickel of 58 - 68.9 % |
Niobium | 3.2 - 4.2 % Show Material materials with Niobium of 3.2 - 4.2 % |
Phosphor | 0 - 0.02 % Show Material materials with Phosphor of 0 - 0.02 % |
Schwefel | 0 - 0.015 % Show Material materials with Schwefel of 0 - 0.015 % |
Silizium | 0 - 0.5 % Show Material materials with Silizium of 0 - 0.5 % |
Titan | 0 - 0.4 % Show Material materials with Titan of 0 - 0.4 % |