Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | O | |
2.705 g/cm³ Show Material materials with Dichte of 2.705 g/cm³ | O | AA Standards |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Dehnung | 23.0 % Show Material materials with Dehnung of 23.0 % | O | ||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | O | AA Standards | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||
Schubmodule | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | Typical for Wrought 1000 Series Aluminium | ||
Streckgrenze | 29.0 MPa Show Material materials with Streckgrenze of 29.0 MPa | O | ||
30.0 MPa Show Material materials with Streckgrenze of 30.0 MPa | O | AA Standards | RP02 | |
Zugfestigkeit | 78.0 MPa Show Material materials with Zugfestigkeit of 78.0 MPa | O | ||
85.0 MPa Show Material materials with Zugfestigkeit of 85.0 MPa | O | AA Standards |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | O | |||
20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | O | AA Standards | ||
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | O | AA Standards | ||
Schmelzpunkt | 645.0 - 655.0 °C Show Material materials with Schmelzpunkt of 645.0 - 655.0 °C | O | AA Standards | ||
650.0 °C Show Material materials with Schmelzpunkt of 650.0 °C | O | ||||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | O | |||
Wärmeleitfähigkeit | 230.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 230.0 W/(m·K) | O | |||
23 °C | 234 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 234 W/(m·K) | O | AA Standards | unstated value |
Elektrisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Elektrische Leitfähigkeit | 36000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 36000000.0 S/m | O | AA Standards | |
spezifischer Widerstand | 2.78e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.78e-08 Ω·m | O | AA Standards | |
2.79e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.79e-08 Ω·m | O | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 99.5 % Show Material materials with Aluminium of 99.5 % | O | AA Standards |
99.5 - 100.0 % Show Material materials with Aluminium of 99.5 - 100.0 % | O | ||
Andere | 0.1 % Show Material materials with Andere of 0.1 % | O | |
Bor | 0.05 % Show Material materials with Bor of 0.05 % | O | AA Standards |
Chrom | 0.01 % Show Material materials with Chrom of 0.01 % | O | AA Standards |
Eisen | 0.40 % Show Material materials with Eisen of 0.40 % | O | AA Standards |
0.4 % Show Material materials with Eisen of 0.4 % | O | ||
Gallium | 0.03 % Show Material materials with Gallium of 0.03 % | O | AA Standards |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | O | AA Standards |
Mangan | 0.01 % Show Material materials with Mangan of 0.01 % | O | AA Standards |
Silizium | 0.1 % Show Material materials with Silizium of 0.1 % | O | AA Standards |
Titan | 0.02 % Show Material materials with Titan of 0.02 % | O | |
Vanadium | 0.02 % Show Material materials with Vanadium of 0.02 % | O | |
Zink | 0.05 % Show Material materials with Zink of 0.05 % | O | AA Standards |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12, H111), poor (H14, H24, H16, H26, H18) | |
Workability | general (condition): good (O, H12, H111, H14, H24), acceptable (H16, H26, H18) |