Allgemein
Property | Value | Condition |
---|---|---|
Dichte | 3.1 g/cm³ Show Material materials with Dichte of 3.1 g/cm³ | T4 |
Mechanisch
Property | Value | Condition | Comment |
---|---|---|---|
Charpy impact energy, V-notch | 21.7 J Show Material materials with Charpy impact energy, V-notch of 21.7 J | T4 | |
Dehnung | 20.0 % Show Material materials with Dehnung of 20.0 % | T4 | |
20 % Show Material materials with Dehnung of 20 % | T4 | Sand cast, elongation in 50 mm | |
Elastizitätsmodul | 71.0 GPa Show Material materials with Elastizitätsmodul of 71.0 GPa | T4 | |
71 GPa Show Material materials with Elastizitätsmodul of 71 GPa | T4 | ||
Härte, Brinell | 95 [-] Show Material materials with Härte, Brinell of 95 [-] | T4 | 500 kg load, 10 mm b |
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | T4 | |
Schubmodule | 23.0 GPa Show Material materials with Schubmodule of 23.0 GPa | T4 | |
Streckgrenze | 215 MPa Show Material materials with Streckgrenze of 215 MPa | T4 | Sand cast, RP02 |
220.0 MPa Show Material materials with Streckgrenze of 220.0 MPa | T4 | ||
Zugfestigkeit | 365 MPa Show Material materials with Zugfestigkeit of 365 MPa | T4 | Sand cast |
370.0 MPa Show Material materials with Zugfestigkeit of 370.0 MPa | T4 |
Thermisch
Property | Value | Condition |
---|---|---|
Koeffizient der thermischen Ausdehnung | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | T4 |
Schmelzpunkt | 570.0 °C Show Material materials with Schmelzpunkt of 570.0 °C | T4 |
Spezifische Wärmekapazität | 920.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 920.0 J/(kg·K) | T4 |
Wärmeleitfähigkeit | 120.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 120.0 W/(m·K) | T4 |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 16000000.0 - 23000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 16000000.0 - 23000000.0 S/m | Typical for Cast 2xx.x Series Aluminium |
spezifischer Widerstand | 4.347826086956522e-08 - 6.25e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.347826086956522e-08 - 6.25e-08 Ω·m | Typical for Cast 2xx.x Series Aluminium |
Chemical properties
Property | Value | Condition |
---|---|---|
Aluminium | 92.1 - 95.1 % Show Material materials with Aluminium of 92.1 - 95.1 % | T4 |
Andere | 0.1 % Show Material materials with Andere of 0.1 % | T4 |
Eisen | 0.15 % Show Material materials with Eisen of 0.15 % | T4 |
Kupfer | 4.0 - 5.2 % Show Material materials with Kupfer of 4.0 - 5.2 % | T4 |
Magnesium | 0.15 - 0.55 % Show Material materials with Magnesium of 0.15 - 0.55 % | T4 |
Mangan | 0.2 - 0.5 % Show Material materials with Mangan of 0.2 - 0.5 % | T4 |
Silber | 0.4 - 1.0 % Show Material materials with Silber of 0.4 - 1.0 % | T4 |
Silizium | 0.1 % Show Material materials with Silizium of 0.1 % | T4 |
Titan | 0.15 - 0.35 % Show Material materials with Titan of 0.15 - 0.35 % | T4 |