Allgemein
Property | Value | Condition |
---|---|---|
Dichte | 3.1 g/cm³ Show Material materials with Dichte of 3.1 g/cm³ | T7 |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 3.0 % Show Material materials with Dehnung of 3.0 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting | A100 | |
4.4 % Show Material materials with Dehnung of 4.4 % | T7 | |||||
25 °C | 4.5 % Show Material materials with Dehnung of 4.5 % | T7 | Sand cast, elongation in 50 mm | |||
105 °C | 7 % Show Material materials with Dehnung of 7 % | T7 | Sand cast, elongation in 50 mm | |||
205 °C | 14 % Show Material materials with Dehnung of 14 % | T7 | Sand cast, elongation in 50 mm | |||
315 °C | 43 % Show Material materials with Dehnung of 43 % | T7 | Sand cast, elongation in 50 mm | |||
Elastizitätsmodul | 71.0 GPa Show Material materials with Elastizitätsmodul of 71.0 GPa | T7 | ||||
71 GPa Show Material materials with Elastizitätsmodul of 71 GPa | T7 | |||||
Härte, Brinell | 130 [-] Show Material materials with Härte, Brinell of 130 [-] | T7 | 500 kg load, 10 mm b | |||
Kriechfestigkeit | 150 °C | 270 MPa Show Material materials with Kriechfestigkeit of 270 MPa | T7 | up to 1000 hours | ||
175 °C | 180 MPa Show Material materials with Kriechfestigkeit of 180 MPa | T7 | up to 1000 hours | |||
205 °C | 130 MPa Show Material materials with Kriechfestigkeit of 130 MPa | T7 | up to 1000 hours | |||
230 °C | 95 MPa Show Material materials with Kriechfestigkeit of 95 MPa | T7 | up to 1000 hours | |||
260 °C | 70 MPa Show Material materials with Kriechfestigkeit of 70 MPa | T7 | up to 1000 hours | |||
290 °C | 48 MPa Show Material materials with Kriechfestigkeit of 48 MPa | T7 | up to 1000 hours | |||
315 °C | 31 MPa Show Material materials with Kriechfestigkeit of 31 MPa | T7 | up to 1000 hours | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | T7 | ||||
Schubmodule | 23.0 GPa Show Material materials with Schubmodule of 23.0 GPa | T7 | ||||
Streckgrenze | 345.0 MPa Show Material materials with Streckgrenze of 345.0 MPa | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting | RP02 | |
410.0 MPa Show Material materials with Streckgrenze of 410.0 MPa | T7 | |||||
25 °C | 415 MPa Show Material materials with Streckgrenze of 415 MPa | T7 | Sand cast, RP02 | |||
105 °C | 275 MPa Show Material materials with Streckgrenze of 275 MPa | T7 | Sand cast, RP02 | |||
205 °C | 150 MPa Show Material materials with Streckgrenze of 150 MPa | T7 | Sand cast, RP02 | |||
315 °C | 55 MPa Show Material materials with Streckgrenze of 55 MPa | T7 | Sand cast, RP02 | |||
Zugfestigkeit | 415.0 MPa Show Material materials with Zugfestigkeit of 415.0 MPa | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting | ||
470.0 MPa Show Material materials with Zugfestigkeit of 470.0 MPa | T7 | |||||
25 °C | 467 MPa Show Material materials with Zugfestigkeit of 467 MPa | T7 | Sand cast | |||
105 °C | 315 MPa Show Material materials with Zugfestigkeit of 315 MPa | T7 | Sand cast | |||
205 °C | 185 MPa Show Material materials with Zugfestigkeit of 185 MPa | T7 | Sand cast | |||
315 °C | 60 MPa Show Material materials with Zugfestigkeit of 60 MPa | T7 | Sand cast |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | T7 | ||||
100 °C | 0.0000193 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.0000193 1/K | T7 | unstated value between 20°C and the mentioned temperature | |||
200 °C | 0.0000227 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.0000227 1/K | T7 | unstated value between 20°C and the mentioned temperature | |||
300 °C | 0.0000247 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.0000247 1/K | T7 | unstated value between 20°C and the mentioned temperature | |||
Schmelzpunkt | 570.0 °C Show Material materials with Schmelzpunkt of 570.0 °C | T7 | ||||
571.0 - 649.0 °C Show Material materials with Schmelzpunkt of 571.0 - 649.0 °C | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |||
Spezifische Wärmekapazität | 920.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 920.0 J/(kg·K) | T7 | ||||
Wärmeleitfähigkeit | 120.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 120.0 W/(m·K) | T7 |
Elektrisch
Property | Value | Condition | Comment |
---|---|---|---|
Elektrische Leitfähigkeit | 19000000 S/m Show Material materials with Elektrische Leitfähigkeit of 19000000 S/m | T7 | Typical/Derived values |
Specific Electrical conductivity | 32.0 - 34.0 % IACS Show Material materials with Specific Electrical conductivity of 32.0 - 34.0 % IACS | T7 | Typical values |
spezifischer Widerstand | 4.347826086956522e-08 - 6.25e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.347826086956522e-08 - 6.25e-08 Ω·m | Typical for Cast 2xx.x Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 92.1 - 95.1 % Show Material materials with Aluminium of 92.1 - 95.1 % | T7 | ||
Andere | 0.1 % Show Material materials with Andere of 0.1 % | T7 | ||
Eisen | 0.15 % Show Material materials with Eisen of 0.15 % | T7 | ||
0.15 % Show Material materials with Eisen of 0.15 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
Kupfer | 4.0 - 5.2 % Show Material materials with Kupfer of 4.0 - 5.2 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Magnesium | 0.15 - 0.55 % Show Material materials with Magnesium of 0.15 - 0.55 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Mangan | 0.2 - 0.5 % Show Material materials with Mangan of 0.2 - 0.5 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Silber | 0.4 - 1.0 % Show Material materials with Silber of 0.4 - 1.0 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Silizium | 0.1 % Show Material materials with Silizium of 0.1 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Titan | 0.15 - 0.35 % Show Material materials with Titan of 0.15 - 0.35 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |